A method for preparing graphene-doped silicon-carbon material

Through the bidirectional modified graphene doping method, a porous carbon material with high conductivity and high mechanical properties is formed, which solves the problem of insufficient electrochemical performance of silicon carbon anode material under low temperature conditions, and significantly improves the electrochemistry of lithium-ion batteries. Performance and cycle life.

CN118763211BActive Publication Date: 2024-11-05BEIJING IAMETAL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254858.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-05
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing silicon-carbon anode materials have poor electrochemical performance under low temperature conditions, and the interface binding capacity of silicon nanoparticles and porous carbon are insufficient, resulting in limited use of lithium-ion batteries at low temperatures.

Method used

Using a bidirectional modified graphene doping method, the porous carbon material with high conductivity and high mechanical properties is formed by mixing dopants in aqueous alcohol solution, sonication, reaction, curing and pyrolytic activation, and the Silicon nanoparticles are deposited on the surface and carbon coating are carried out to enhance the interface binding ability of the silicon nanoparticles and porous carbon.

Benefits of technology

It significantly improves the electrochemical performance of lithium-ion batteries, especially its performance under low temperature conditions, extends the cycle life of the battery and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763211B_ABST
    Figure CN118763211B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a graphene-doped silicon-carbon composite material, comprising the following steps: after graphene is doped with NP, it is subjected to bidirectional modification by hydrogen peroxide and ammonia water, and hydrazine hydrate to obtain modified graphene, the modified graphene is dispersed in a polymer resin solution, and solidification, pyrolysis, activation, silicon nanoparticle deposition, and carbon coating are sequentially performed to obtain a product graphene-doped silicon-carbon composite material. The graphene-doped silicon-carbon material prepared by the present invention enhances the overall electrical conductivity and mechanical properties of the silicon-carbon material, enhances the interface bonding ability between silicon nanoparticles and carbon matrix, inhibits the repeated volume changes of silicon nanoparticles in subsequent cycles, resulting in the detachment from the carbon matrix, and ensures the cycle performance of the battery. Therefore, the graphene-doped porous carbon prepared by the present invention provides a high-performance carbon matrix, which has excellent electrochemical properties when applied to lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a method for preparing a graphene-doped silicon-carbon material. Background Art

[0002] In recent years, the steady growth of electric vehicle endurance and grid energy storage needs has continuously challenged the energy limit of lithium-ion batteries. Among them, replacing the traditional graphite anode with high-capacity materials is the most promising way to achieve higher energy density lithium-ion batteries. Silicon anode has a high theoretical capacity (Li 4.4 Si is 4200 mAh g -1 , 10 times higher than graphite), moderate voltage platform (0.4 V vs Li + / Li), abundant reserves and environmental friendliness, it is considered to be a highly competitive candidate material. However, due to the huge volume fluctuations during the (de)lithiation process, the silicon anode suffers from severe structural degradation and instability of the solid electrolyte interface (SEI). These problems not only lead to particle rupture of the active material and poor contact with the electrode, but also mechanically disrupt the stable formation of the SEI layer and continuously expose the new surface of the material to the electrolyte. In addition, the poor intrinsic electronic conductivity of silicon also leads to slow electrochemical kinetics.

[0003] In response to the above-mentioned silicon negative electrode volume expansion problem, domestic and foreign scholars have invested a lot of research, among which new silicon-carbon materials stand out on the road to commercialization due to their high initial efficiency and long cycle life. Generally, new silicon-carbon materials use CVD vapor deposition technology to deposit nanosilicon in porous carbon materials with developed pore structures. Porous carbon, as a substrate material, is a good carrier for silicon nucleation and growth. Its developed pore structure is conducive to expanding the specific surface area of ​​the silicon negative electrode, thereby improving the electrochemical activity of the electrode. At the same time, the conductivity and mechanical stability of porous carbon are directly related to the overall performance of the silicon negative electrode. Therefore, it is urgent to develop a porous carbon material with high conductivity, high mechanical properties, and strong interfacial bonding with silicon to improve the electrochemical performance of new silicon-carbon negative electrode materials. The prior art has improved its electrochemical performance by doping silicon-carbon composite negative electrode materials. For example, CN115832264A, CN117963931A, and CN117855423A, in which the silicon-carbon negative electrode material doped with graphene has excellent electrochemical properties and has attracted much attention. For example, CN118335960A discloses a method for preparing a porous silicon-carbon composite negative electrode material, which includes the following steps: S1, placing composite diatomaceous earth in a closed quartz tube, raising the temperature of the quartz tube to 700-780°C at a heating rate of 5-8°C / min in a mixed gas atmosphere, and heat-preserving the tube for 12-14 hours, and then post-treating the nano-composite silicon; S2, coating a layer of graphene on the outside of the nano-composite silicon to prepare composite nano-silicon; S3, placing polyvinylidene chloride on the surface of the nano-composite silicon; , polyvinyl butyral, and N,N-dimethylformamide are added to the reactor and stirred until the system is dissolved, composite nano-silicon is added to the reactor, the temperature of the reactor is increased to 55-65°C, stirred for 2-3 hours, and post-treated to obtain a silicon-carbon composite precursor; S4, the silicon-carbon composite precursor is added to a tubular furnace protected by an inert gas atmosphere, the temperature of the tubular furnace is increased to 720-750°C, heat-insulated for 6-8 hours, cooled, discharged, ground, and passed through a 200-mesh sieve to obtain a silicon-carbon composite material. CN118099362A discloses a method for preparing a silicon-carbon negative electrode, comprising the following steps: (1) mixing organic silicon with a dispersant, graphene, and a nitrogen dopant, evacuating the mixture, and subjecting the mixture to ultrasonic treatment for 2-5 hours; (2) adding powdered asphalt after the ultrasonic treatment, mixing the mixture, and heating the mixture to a temperature of 120-300°C, and mixing and crushing the mixture again in a strong shearing device to obtain a silicon-carbon negative electrode precursor powder; (3) carbonizing the silicon-carbon negative electrode precursor powder at a high temperature of 500-1000°C for 8-10 hours under the protection of an inert gas, and cooling the mixture to obtain a silicon-carbon negative electrode material.CN117963931A discloses a method for preparing a highly conductive silicon-carbon negative electrode material for a lithium-ion battery, comprising the following steps: (1) uniformly mixing SiO2 and a phosphorus source, and calcining at high temperature to obtain a phosphorus-doped silicon precursor; (2) uniformly mixing the phosphorus-doped silicon precursor obtained in step (1) with magnesium powder, reducing at high temperature, and after cooling the reaction, successively immersing the product in hydrochloric acid and hydrofluoric acid solutions to remove by-products, centrifugally collecting, and vacuum drying to obtain a defect-modified nano-silicon material; (3) treating the defect-modified nano-silicon material prepared in step (2) with graphene in a high-energy ball mill to obtain a silicon-carbon negative electrode material with high conductivity. CN116053436A discloses a method for preparing a nitrogen-doped graphene silicon-carbon composite material, comprising the following steps: S1, dispersing nano-silicon, a dispersant, and a binder into deionized water, drying, and heat-treating the obtained solid matter in a mixed atmosphere of an inert gas and oxygen to obtain carboxylated nano-silicon particles; S2, adding the carboxylated nano-silicon particles to a dopamine solution, introducing oxygen to carry out a polymerization reaction, and performing solid-liquid separation to obtain a nano-silicon / polydopamine composite material; S3, adding the nano-silicon / polydopamine composite material to a graphene oxide solution, performing a hydrothermal treatment, performing solid-liquid separation, and drying to obtain a nano-silicon / polydopamine / graphene oxide composite material; S4, heating the nano-silicon / polydopamine / graphene oxide composite material once and keeping it warm once in a hydrogen atmosphere, and then heating it twice and keeping it warm twice to obtain the nitrogen-doped graphene silicon-carbon composite material. CN116544376A reports a method for preparing a low-expansion silicon-carbon material, comprising the following steps: S1, adding silicon-oxygen compounds, graphene oxide solution, and organic metal polymers to an organic carbon source solution, spray drying, and then reacting at 100-200°C and 1-5Mpa for 1-6h to obtain a graphene oxide-coated metal-doped silicon-oxygen precursor material; S2, introducing a mixed gas of a boron source gas and argon gas into the graphene oxide-coated metal-doped silicon-oxygen precursor material to react and obtain a boron-doped silicon-carbon composite material; S3, soaking the boron-doped silicon-carbon composite material in a hydrofluoric acid solution, and drying to obtain a low-expansion silicon-carbon material. However, the above patents do not combine well with the carbon matrix, resulting in poor electrochemical performance, especially poor electrochemical performance at low temperatures, which affects the use of batteries under low temperature conditions. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a graphene-doped silicon-carbon material, by giving graphene excellent conductivity and different surface polar groups through bidirectional modification, then uniformly dispersing the modified graphene in a resin solution, and performing pyrolysis, activation, silane deposition, and carbon coating steps after curing, so that the prepared porous carbon material has high conductivity and high mechanical properties. At the same time, the different polar groups on the surface of the modified graphene will enhance the interfacial bonding ability between silicon nanoparticles and porous carbon, thereby providing the required high-performance porous carbon matrix for the silicon-carbon material, improving the electrochemical properties of lithium-ion batteries, especially the electrochemical properties at low temperatures.

[0005] A method for preparing a graphene-doped silicon-carbon composite material comprises the following steps:

[0006] (S1) Graphene and a dopant are uniformly mixed in an alcohol aqueous solution, and freeze-dried to obtain doped graphene; the dopant contains N and P elements;

[0007] (S2) adding the doped graphene into a mixed solution of hydrogen peroxide and ammonia, ultrasonically treating, washing, and drying;

[0008] (S3) dispersing the dried material into an alcohol aqueous solution, adding hydrazine hydrate, heating to react, washing, and drying to obtain modified graphene;

[0009] (S4) dispersing the modified graphene into a polymer resin solution, heating and curing the solution, and crushing and drying the product obtained after cooling to obtain a cured material;

[0010] (S5) pyrolyzing and activating the solidified material to obtain a doped porous carbon material;

[0011] (S6) The doped porous carbon material is sequentially subjected to silicon nanoparticle deposition and carbon coating to obtain a graphene-doped silicon-carbon composite material.

[0012] Furthermore, in step (S1), the type of graphene is one or more combinations of single-layer graphene, double-layer graphene, and multi-layer graphene; and the dopant is selected from at least one of ammonium phosphate, diammonium dihydrogen phosphate, and diammonium hydrogen phosphate.

[0013] Furthermore, in step (S1), the mass ratio of the dopant to the graphene is 1:1-2.

[0014] Furthermore, in step (S1), the alcohol aqueous solution is a mixed solution of C1-3 alcohol and water in a volume ratio of 1-2:1-2, and the C1-3 alcohol is selected from at least one of methanol, ethanol, and isopropanol; and the freeze-drying is carried out at 1Pa-100Pa and -30°C to -20°C.

[0015] Furthermore, in step (S2), the concentration of hydrogen peroxide is 20-30wt%, the concentration of ammonia water is 20-25wt%, the volume ratio of hydrogen peroxide to ammonia water is 3-5:3-5, and the ratio of the mass of doped graphene to the volume of the mixed solution of hydrogen peroxide and ammonia water is 1g:100-160mL; the ultrasonic treatment is carried out at 60-100kHz for 3-5h, and the washing is carried out with deionized water until neutral; there is no special limitation on drying, such as vacuum drying.

[0016] Furthermore, in step (S3), the alcohol-water solution is a mixed solution of C1-3 alcohol and water in a volume ratio of 1-2:1-2, the ratio of the mass of the dried material to the volume of the alcohol-water solution is 1-3g:100mL; the ratio of the mass of the dried material to the volume of hydrazine hydrate is 1g:3-5mL; the temperature reaction is 70-90°C for 5-10h; the washing is 3-5 times of alternating washing with ethanol and deionized water, and there is no special limitation on drying, such as vacuum drying.

[0017] Furthermore, in step (S4), the polymer resin is selected from at least one of epoxy resin, phenolic resin, vinyl resin, melamine-formaldehyde resin, and acrylic resin, the solid content of the liquid polymer resin solution is 30-60wt%, and the solvent is selected from at least one of water, ethanol, acetone, toluene, and ethyl acetate.

[0018] Furthermore, in step (S4), the mass ratio of modified graphene to polymer resin solution is 1-5:100, preferably 2-4:100; dispersion is stirring under ultrasonic conditions, the ultrasonic frequency is 60-100kHz, and stirring is stirring at a speed of 300-500rpm for 0.5-1h; heating curing is transferring the evenly dispersed solution to a water heating box and curing it at a constant temperature of 80-100°C for 15-24h, and crushing is crushing to a material with a median particle size of 2-50μm, preferably 5-20μm, and the crushing method is not particularly limited, such as air flow crushing.

[0019] Further, in step (S5), pyrolysis is carried out under a protective atmosphere, the pyrolysis temperature is 500-800°C, the heating rate is 5°C / min-10°C / min, and after heating to the pyrolysis temperature, it is kept warm for 1-3 hours, and the protective atmosphere is nitrogen and / or argon. The activation method is physical activation or chemical activation. Preferably, physical activation is carried out in an active atmosphere, the activation temperature is 600-1000°C, the heating rate is 2°C / min-10°C / min, the activation time is 4-10 hours, and the active atmosphere is one or more combinations of CO2, water vapor or air atmosphere; chemical activation is heat treatment after pyrolysis carbon and activator are uniformly mixed; the activator is one or more combinations of zinc chloride, calcium chloride, potassium carbonate, phosphoric acid, potassium dihydrogen phosphate, potassium sulfide, sulfuric acid, potassium hydroxide, sodium hydroxide, and boric acid; the heat treatment temperature is 400-800°C, the heating rate is 2°C / min-10°C / min, and the holding time is 5-8 hours.

[0020] Further, in step (S6), the silicon nanoparticle deposition method is to contact the doped porous carbon material with a silicon source gas under heating conditions, specifically, the doped porous carbon material is placed in the heating zone of a rotary kiln, the original air is exhausted, and the silicon source gas is introduced into the rotary kiln while the temperature is uniformly increased, and the silicon source is chemically vapor deposited to obtain graphene-doped porous carbon with deposited silicon-based nanoparticles; the silicon nanoparticles are one or more combinations of silicon, silicon dioxide, and silicon dioxide nanoparticles, accounting for 30-60wt% of the graphene-doped silicon-carbon composite material, preferably 40-50%. The silicon nanoparticles are present in the pores of the graphene-doped porous carbon. Preferably, the silicon source gas is a combination of one or more silicon source gases of monosilane, disilane, tetrafluorosilane, dichlorosilane, and hexamethyldisilane. The silicon nanoparticle deposition temperature is 600-1200°C, the deposition time is 6-12h, and the rotary kiln speed is 2r / min-5r / min.

[0021] Preferably, in step (S6), the carbon coating method is to contact the graphene-doped porous carbon deposited with silicon-based nanoparticles with a carbon source gas under heating conditions. Specifically, the temperature of the rotary kiln is uniformly increased in the atmosphere of protective gas, and a mixed gas of the carbon source gas and the protective gas is introduced, and the graphene-doped porous carbon deposited with silicon nanoparticles is subjected to carbon coating treatment to obtain the graphene-doped porous carbon-new silicon-carbon material. Preferably, the carbon source gas is one or more combinations of acetylene, methane, propylene, propane, etc., and the carbon coating layer is uniformly distributed on the outermost surface of the graphene-doped porous carbon deposited with silicon nanoparticles, the carbon coating temperature is 550~950℃, the coating time is 1~5 h, and the thickness of the carbon coating layer is 5~10 nm.

[0022] The graphene-doped silicon-carbon material provided by the present invention is applied to the preparation of electrode materials in a battery system.

[0023] The graphene-doped silicon-carbon material proposed in the present invention enhances the overall conductivity and mechanical properties of the silicon-carbon material by doping and bidirectionally modifying graphene, enhances the interface bonding ability between silicon nanoparticles and the carbon matrix, inhibits the repeated volume changes of silicon nanoparticles in subsequent cycles that cause them to fall off the carbon matrix, and ensures the cycle performance of the battery. Therefore, the graphene-doped porous carbon prepared by the present invention provides a high-performance carbon matrix, which has excellent electrochemical properties when applied to lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the SEM image of the silicon-carbon material prepared in Example 1;

[0025] Figure 2 TEM image of the silicon-carbon material prepared in Example 1;

[0026] Figure 3 This is the first cycle charge and discharge curve of the silicon-carbon material prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention is further described below through the accompanying drawings and specific embodiments, but it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the protection scope of the present invention.

[0028] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0029] Example 1

[0030] (S1) Graphene powder and ammonium dihydrogen phosphate were uniformly mixed in a mass ratio of 1:1 in deionized water and anhydrous ethanol (v / v, 1:1) and stirred under magnetic stirring at 300 rpm for 1 hour. The mixed solution was then freeze-dried in vacuum for 4 hours to obtain N and P doped graphene.

[0031] (S2) 1.5 g of N, P-doped graphene powder was added to 240 ml of a mixed solution of hydrogen peroxide (30 wt%) and ammonia water (25 wt%) in a volume ratio of 3:5 at room temperature with stirring. The solution was then ultrasonically treated at 100 kHz for 4 h, filtered, washed with deionized water until neutral, and dried in a vacuum oven at 60 °C for 12 h.

[0032] (S3) 1 g of the dried material was dispersed in 100 mL of ethanol-water solution (alcohol concentration 60 vol%), 3 mL of hydrazine hydrate was slowly added dropwise, and the temperature was raised to 80 ° C for reaction for 6 h. After the reaction was completed, it was cooled to room temperature and filtered. The filter cake was washed alternately with deionized water and ethanol three times, and dried in a vacuum oven at 60 ° C for 12 h to obtain modified graphene;

[0033] (S4) The modified graphene powder was stirred and dispersed into a phenolic resin aqueous solution with a solid content of 60% at a mass fraction, stirred at a speed of 350 r / min for 30 min, and then ultrasonicated at 100 kHz for 4 h to make it uniformly dispersed in the phenolic resin solution. The mixed solution was then transferred to a water heating box and cured at a constant temperature of 90° C. for 16 h. The mixed solution was crushed by a crusher to a median particle size of about 10 μm, and dried in a vacuum oven at 90° C. for 24 h to obtain a cured material.

[0034] (S5) The solidified material is placed in a pyrolysis rotary furnace with good airtightness, and the temperature is increased to 750°C at a heating rate of 8°C / min in a N2 atmosphere, and the temperature is kept at this temperature for 3 hours to obtain pyrolytic carbon; the pyrolytic carbon is placed in an activation rotary furnace, and the temperature is increased to 1000°C at a heating rate of 3°C / min in a CO2 atmosphere, and the temperature is kept at this temperature for 9 hours to obtain a doped porous carbon material;

[0035] (S6) The doped porous carbon material is placed in a rotary furnace. While continuously passing an Ar atmosphere for protection, monosilane gas is continuously introduced. The temperature is raised to 900°C at a heating rate of 2°C / min and kept at this temperature for 9 hours so that the silicon nanoparticles are uniformly deposited in the pores of the porous carbon in the mixed gas. After chemical vapor deposition for 12 hours, modified graphene-doped porous carbon with deposited silicon nanoparticles is obtained, wherein the silicon content is 49%. After the deposition of the nano-silicon particles is completed, the modified graphene-doped porous carbon with deposited silicon nanoparticles is cooled to room temperature, and the modified graphene-doped porous carbon with deposited silicon nanoparticles is transferred to a carbon-coated rotary furnace. In a mixed atmosphere of ethane and N2, the temperature in the furnace is raised to 800°C, and the bidirectional modified graphene-doped porous carbon with deposited silicon nanoparticles is carbon-coated for 2 hours to obtain the graphene-doped porous carbon-new silicon-carbon material, and the carbon coating layer has a thickness of 8 nm.

[0036] Figure 1 This is the SEM image of the silicon-carbon material prepared in Example 1.

[0037] Figure 2 This is the TEM image of the silicon-carbon material prepared in Example 1.

[0038] Figure 3 This is the first cycle charge and discharge curve of the silicon-carbon material prepared in Example 1.

[0039] Example 2

[0040] The other conditions and steps are the same as those in Example 1, except that in step (S1), the mass ratio of graphene powder to ammonium dihydrogen phosphate is 1:2; in step (S2), the amount of the mixed solution of hydrogen peroxide and ammonia water is changed to 100 mL; in step (S3), the amount of hydrazine hydrate added is changed to 5 mL.

[0041] Example 3

[0042] The other conditions and steps are the same as those in Example 1, except that in step (S4), the modified graphene powder is stirred and dispersed into a 60% phenolic resin solution at a mass fraction of 4%.

[0043] Example 4

[0044] The other conditions and steps are the same as those in Example 1, except that in step (S4), the modified graphene powder is stirred and dispersed into a 60% phenolic resin solution at a mass fraction of 1%.

[0045] Example 5

[0046] The other conditions and steps are the same as those in Example 1, except that in step (S4), the modified graphene powder is stirred and dispersed into a 60% phenolic resin solution at a mass fraction of 5%.

[0047] Comparative Example 1

[0048] The other conditions and operations are the same as those in Example 1, except that graphene is not added, that is, steps (S1) to (S3) are cancelled, and step (S4) is changed to: the phenolic resin solution with a solid content of 60% is cured at a constant temperature of 90° C. for 16 h, and then the same as in Example 1.

[0049] Comparative Example 2

[0050] Other conditions and operations are the same as those in Example 1, except that steps (S1) to (S3) are omitted, graphene is not modified, and graphene is directly dispersed by stirring at a mass fraction of 2% into a phenolic resin solution having a solid content of 60%, and then the same as in Example 1.

[0051] Comparative Example 3

[0052] Other conditions and operations are the same as those in Example 1, except that there is no step (S1), and step (S2) is changed to: 1.5 g of graphene powder is added to 240 ml of a mixed solution of hydrogen peroxide (30%) and ammonia water in a volume ratio of 3:5 at room temperature with stirring, then the solution is ultrasonically treated at 100 kHz for 4 h, filtered, washed with deionized water until neutral, dried in a vacuum oven at 60° C. for 12 h, and then the same as in Example 1.

[0053] Comparative Example 4

[0054] Other conditions and operations are the same as those in Example 1, except that there is no step (S2). After step (S1), step (S3) is directly performed: 1 g of the freeze-dried material in step (S1) is dispersed in 100 mL of ethanol-water solution (alcohol concentration 60 vol%), and then the same as in Example 1.

[0055] Comparative Example 5

[0056] Other conditions and operations are the same as those in Example 1, except that there is no step (S3). In step (S2), the vacuum-dried graphene is stirred and dispersed in a phenolic resin solution with a solid content of 60% at a mass fraction of 2%, and then the same as in Example 1.

[0057] Application Examples

[0058] The silicon-carbon materials prepared in the above embodiments and comparative examples were used as negative electrodes to assemble lithium batteries. The battery assembly was carried out in a glove box with a water and oxygen content of less than 0.1 ppm. Taking the button battery CR2032 as an example: two-dimensional doped porous carbon-new silicon-carbon material was used as the active material, super p was used as the conductive agent, and PAA was used as the binder to prepare the slurry, which was coated on the copper foil current collector to form the negative electrode, the lithium sheet was used as the counter electrode, Celgard 2500 was used as the diaphragm, and 1 mol / L LiPF6 (volume ratio EC:DMC:DEC=1:1:1, with an additional 5% volume of FEC) was used as the electrolyte to assemble the battery. The electrochemical performance test was carried out at a constant temperature of 25°C, with a test voltage range of 0.005-1.5 V and a 0.1 C constant rate charge and discharge test. The results are shown in Table 1 below:

[0059] Table 1 Negative electrode performance test results of the embodiments and comparative examples

[0060] .

[0061] It can be seen from Table 1 that the graphene-doped porous carbon-new silicon-carbon material prepared by the present invention has more excellent electrochemical performance. The embodiment adopts different types of modified graphene to dope the porous carbon material, and uses it as a substrate to prepare a new silicon-carbon material. Comparative Example 1 does not add graphene, and the electrochemical performance is significantly reduced. Comparative Example 2 graphene is not modified. Although the electrochemical performance is improved compared with Comparative Example 1, it is still not as good as the embodiment. The silicon-carbon material prepared in the embodiment not only has a better reversible specific capacity, but also can maintain a higher capacity retention rate at low temperature and high rate. This is because the pure porous carbon material lacks electrical conductivity and mechanical properties, which makes the silicon-carbon material silicon nanoparticles change greatly in volume during the subsequent cycle process, which will cause the negative electrode structure to be destroyed, so that the battery capacity retention rate is reduced; directly doping graphene, although the performance is improved, but the improvement is prioritized, especially the electrochemical performance at low temperature is limited, which is not conducive to the use of actual batteries. The advantages of the modified graphene-doped silicon-carbon material are prominent, with more excellent capacity retention and rate performance, which can not only improve the overall conductivity of the new silicon-carbon material, but also enhance the interfacial bonding ability of silicon nanoparticles and porous carbon materials in the subsequent silicon nanoparticle deposition process, inhibit the particle pulverization caused by the repeated volume changes of silicon in the cycle, and thus alleviate its shedding from the carbon matrix. Comparative Examples 3-5 show that the steps of graphene doping and modification are indispensable in the present invention, otherwise the purpose of graphene doping to improve the electrochemical performance of silicon-carbon composite materials cannot be fully achieved.

Claims

1. A method for preparing a graphene-doped silicon-carbon composite material, characterized in that: The following steps are involved: (S1) Graphene and a dopant are uniformly mixed in an alcohol aqueous solution, and freeze-dried to obtain doped graphene; the dopant contains N and P elements; (S2) adding the doped graphene into a mixed solution of hydrogen peroxide and ammonia, ultrasonically treating, washing, and drying; (S3) dispersing the dried material into an alcohol aqueous solution, adding hydrazine hydrate, heating to react, washing, and drying to obtain modified graphene; (S4) dispersing the modified graphene into a polymer resin solution, heating and curing the solution, and crushing and drying the product obtained after cooling to obtain a cured material; (S5) pyrolyzing and activating the solidified material to obtain a doped porous carbon material; (S6) The doped porous carbon material is sequentially subjected to silicon nanoparticle deposition and carbon coating to obtain a graphene-doped silicon-carbon composite material.

2. The preparation method according to claim 1, characterized in that: In step (S1), the type of graphene is one or more combinations of single-layer graphene, double-layer graphene, and multi-layer graphene; the dopant is selected from at least one of ammonium phosphate, diammonium dihydrogen phosphate, and diammonium hydrogen phosphate; and the mass ratio of the dopant to the graphene is 1:1-2.

3. The preparation method according to claim 1, characterized in that: In step (S1), the alcohol aqueous solution is a mixed solution of C1-3 alcohol and water in a volume ratio of 1-2:1-2, and the C1-3 alcohol is selected from at least one of methanol, ethanol, and isopropanol; and the freeze-drying is carried out at 1Pa-100Pa and -30°C to -20°C.

4. The preparation method according to claim 1, characterized in that: In step (S2), the concentration of hydrogen peroxide is 20-30wt%, the concentration of ammonia water is 20-25wt%, the volume ratio of hydrogen peroxide to ammonia water is 3-5:3-5, and the ratio of the mass of doped graphene to the volume of the mixed solution of hydrogen peroxide and ammonia water is 1g:100-160mL.

5. The preparation method according to claim 1, characterized in that: In step (S3), the alcohol aqueous solution is a mixed solution of C1-3 alcohol and water in a volume ratio of 1-2:1-2, the ratio of the mass of the dried material to the volume of the alcohol aqueous solution is 1-3g:100mL; the ratio of the mass of the dried material to the volume of hydrazine hydrate is 1g:3-5mL; The temperature reaction is 70-90°C for 5-10 hours.

6. The preparation method according to claim 1, characterized in that: In step (S4), the polymer resin is selected from at least one of epoxy resin, phenolic resin, vinyl resin, melamine-formaldehyde resin, and acrylic resin, the solid content of the liquid polymer resin solution is 30-60wt%, and the solvent is selected from at least one of water, ethanol, acetone, toluene, and ethyl acetate.

7. The preparation method according to claim 1, characterized in that: In step (S4), the mass ratio of modified graphene to polymer resin solution is 2-4:100; the temperature curing is to transfer the evenly dispersed solution to a water heating box and cure it at a constant temperature of 80-100° C. for 15-24 hours; The crushing is to crush the material to a median particle size of 2-50 μm.

8. The preparation method according to claim 1, characterized in that: In step (S5), pyrolysis is carried out under a protective atmosphere at a temperature of 500-800°C, and after heating to the pyrolysis temperature, the temperature is maintained for 1-3 hours; and / or The activation method is physical activation or chemical activation.

9. The preparation method according to claim 1, characterized in that: In step (S6), the silicon nanoparticles are deposited by contacting the doped porous carbon material with a silicon source gas under heating conditions, and the silicon nanoparticles account for 30-60wt% of the graphene-doped silicon-carbon composite material; and / or The carbon coating method is to deposit graphene-doped porous carbon of silicon-based nanoparticles in contact with a carbon source gas under heating conditions; the thickness of the carbon coating layer is 5~10 nm.

10. A graphene-doped silicon-carbon composite material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 9.