Silicon negative electrode material for in-situ generation of electrolyte additive and preparation method of silicon negative electrode material

Through the preparation method of in-situ generation of electrolyte additives, magnesium nitride and lithium are used to build a conductive network, which solves the problems of volume change and low ion conductivity of silicon-based lithium-ion batteries during cycling, and achieves high specific capacity and long cycle stability. The coulombic efficiency in the first cycle reaches over 94%, and the process is simple and low-cost.

CN118763213AInactive Publication Date: 2024-10-11NANJING HANJING ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410861094.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon-based lithium-ion batteries have stability and efficiency problems due to volume changes and low ion electronic conductivity during cycling. In particular, solid electrolyte interface films are easily formed at low lithiation potentials, resulting in Coulombic efficiency and capacity fading.

Method used

Using the preparation method of in-situ generation of electrolyte additives, Si, Super-P and Mg3N2 are mixed in a glove box filled with argon and ball milled under an inert gas atmosphere to form magnesium nitride and lithium nitride to build high ion conductivity High-efficiency conductive network, reducing side reactions and improving Coulombic efficiency.

Benefits of technology

The cycle stability and specific capacity of silicon-based lithium-ion batteries have been significantly improved. The Coulombic efficiency of the first cycle has reached more than 94%. The process is simple and low-cost, and the long-term cycle stability has been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763213A_ABST
    Figure CN118763213A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon negative electrode material for in-situ generation of an electrolyte additive and a preparation method thereof, and belongs to the field of lithium ion battery negative electrode materials, the method comprises the following steps: uniformly grinding Si, Super-P and Mg3N2 according to a certain mass ratio to obtain a mixture; placing the mixture in a ball milling tank for ball milling in an inert gas atmosphere; the silicon negative electrode material for in-situ generation of the electrolyte additive is obtained. Li3N and Mg are formed in situ in the circulation process of Mg3N2, Li3N has high ionic conductivity, rapid lithium ion diffusion can be achieved, meanwhile, Mg is a lithium-loving element, an additional point location is provided for diffusion of lithium ions, and an ionic conductive network is constructed. The silicon-based negative electrode material of the lithium ion battery has high specific capacity, side reaction is reduced in the circulation process, the coulombic efficiency of the first circle is improved to 94% or above, meanwhile, the long circulation stability is obviously improved, and the silicon-based negative electrode material can be suitable for commercialized production of the high-specific-energy negative electrode of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium ion battery negative electrode materials, and in particular relates to a silicon negative electrode material for in-situ generation of an electrolyte additive and a preparation method thereof. Background Art

[0002] All-solid-state batteries are regarded as the next generation of energy storage devices due to their higher safety and energy density. The negative electrode material determines the energy density of all-solid-state batteries. Lithium metal and silicon have become two very attractive negative electrode materials due to their ultra-high energy density. The application of lithium metal negative electrodes has greatly improved the energy density of batteries. However, the use of lithium metal in all-solid-state batteries faces many challenges, such as interface instability and the formation of lithium dendrites. Therefore, silicon has been widely explored as a typical alloy type and has become a potential negative electrode material. Silicon has a super theoretical specific capacity, which is about ten times that of traditional graphite. The average reduction potential is about 0.4 V (Vs Li + / Li), preventing the formation of lithium dendrites. Furthermore, silicon is abundant on Earth and very cheap. Despite this, silicon-based lithium-ion batteries still face several challenges. Silicon's significant volume change during cycling and its low ionic and electronic conductivity limit its practical application.

[0003] To address these issues, solid-state electrolytes and conductive agents are often added to electrodes to construct a conductive network. Currently, sulfide electrolytes are widely used in all-solid-state silicon-based lithium-ion batteries due to their extremely high room-temperature ionic conductivity. However, silicon and sulfide electrolytes are unstable at low lithiation potentials and easily form a solid electrolyte interface (SEI). This occurs when sulfide decomposition products and silicon suboxide on the surface of silicon particles undergo disproportionation during physical and chemical processes and enter the SEI, leading to increased polarization, low coulombic efficiency, and rapid capacity decay. Therefore, there is an urgent need to redesign the negative electrode structure of silicon-based lithium-ion batteries. Summary of the Invention

[0004] The present invention provides a silicon negative electrode material with an in-situ generated electrolyte additive and a preparation method thereof, so that the silicon-based negative electrode material of lithium-ion batteries has a high specific capacity, reduces side reactions during the cycle, increases the first-cycle coulombic efficiency to more than 94%, and significantly improves the long-cycle stability. In addition, the process is simple and the cost is low, providing an option for the design of silicon-based negative electrode structures.

[0005] A silicon negative electrode material for in-situ generation of electrolyte additives and a preparation method thereof, comprising the following steps: (1) Si, Super-P, and Mg3N2 were mixed in a glove box filled with argon gas in a certain mass ratio to obtain a mixture; (2) ball milling the mixture under an inert gas atmosphere to obtain a silicon anode material with in-situ generated electrolyte additives; In the above steps, the mass ratio of Si, Super-P and Mg3N2 in step (1) is (30-80):10: (60-10). The mass ratio of Si, Super-P and Mg3N2 will affect the composition of the electrode structure, thereby affecting the electrochemical properties such as the reversible capacity and coulombic efficiency of the silicon-based lithium-ion battery; The mixing described in step (1) specifically includes the following steps: first, grinding Si and Super-P evenly in a mortar for 15-20 minutes, and then adding Mg3N2 and grinding evenly for 15-20 minutes; first mixing Si and Super-P, Super-P coating on the surface of Si can alleviate the volume expansion of Si during the electrochemical cycle process and improve the conductivity of the electrode material; The inert gas described in step (2) is argon, helium or nitrogen; the ball mill is a planetary ball mill with a ball-to-material ratio of 160:1, a ball mill revolution speed of 200 rpm, and a ball milling time of 30 minutes; ball milling Si, Super-P and Mg3N2 can achieve material mixing, homogenization and dispersion, which is more conducive to subsequent reactions; the setting of the ball-to-material ratio directly affects the ball milling effect. If the ball-to-material ratio is too low, it may lead to poor ball milling effect; if the ball-to-material ratio is too high, the self-wear between the grinding balls will be aggravated, which to a certain extent reduces the interaction between the balls and the materials.

[0006] Beneficial Effects: The present invention provides a silicon anode material with an in-situ electrolyte additive generation method and its preparation method. Lithium nitride and magnesium are formed in situ during the cycling process. Magnesium nitride has high ionic conductivity, enabling rapid lithium ion diffusion. Furthermore, magnesium, a lithium-philic element, provides additional sites for lithium ion diffusion, building an ion-conducting network. This results in a lithium-ion battery silicon-based anode material with high specific capacity, reduced side reactions during cycling, and increased first-cycle coulombic efficiency to over 94%. Long-cycle stability is significantly improved, and the applicable equipment is simple, the process is simple, and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 This is an X-ray diffraction pattern of the silicon negative electrode material with in-situ generated electrolyte additives in an embodiment of the present invention; Figure 2 This is a comparison chart of the reversible capacity of silicon negative electrode materials with in-situ generated electrolyte additives according to an embodiment of the present invention; Figure 3 This is a charge and discharge curve diagram of the silicon negative electrode material with in-situ generated electrolyte additive in Example 4 of the present invention; Figure 4 This is a long cycle diagram of the silicon negative electrode material with in-situ generated electrolyte additives in Example 4 of the present invention. DETAILED DESCRIPTION

[0008] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1

[0009] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 30:10:60 in a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 2

[0010] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 40:10:50 in a mortar, specifically comprising the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 3

[0011] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 50:10:40 in a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 4

[0012] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 60:10:30 in a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 5

[0013] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 70:10:20 in a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 6

[0014] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 80:10:10 in a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled in a planetary ball mill under a high-purity (99.999%) argon atmosphere in a sealed manner at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained. Example 7

[0015] A method for preparing a silicon anode material with an in-situ generated electrolyte additive comprises the following steps: in an argon-filled glove box, first mixing Si, Super-P, and Mg3N2 in a mass ratio of 90:5:5 using a mortar. Specifically, the method comprises the following steps: first, grinding the Si and Super-P uniformly in the mortar for 15-20 minutes, then adding Mg3N2 and grinding uniformly for 15-20 minutes. The mixture is transferred to a stainless steel ball mill and ball milled using a planetary ball mill. The milling is sealed in a high-purity (99.999%) argon atmosphere at a speed of 200 rpm for 30 minutes, wherein the ball-to-material ratio is 160:1. After ball milling, a silicon anode material with an in-situ generated electrolyte additive is obtained.

[0016] Figure 1 This is the X-ray diffraction pattern of the silicon negative electrode material with in-situ generated electrolyte additive obtained in Example 1-7. It can be found that Si, Super-P and Mg3N2 did not react during the ball milling process.

[0017] Figure 2 The comparison chart of the reversible capacity of the silicon negative electrode material with in-situ generated electrolyte additives obtained in Examples 1 to 7 is shown in FIG. Figure 2 From the comparison, it can be found that the sample obtained in Example 4 has the highest reversible capacity and the best effect, which shows that a good conductive network has been constructed, which is beneficial to the electrode reaction kinetics process.

[0018] Figure 3 This is a charge and discharge curve of the silicon negative electrode material with in-situ generated electrolyte additive obtained in Example 4. The first cycle coulombic efficiency reaches 94.56%, indicating that side reactions are significantly reduced.

[0019] Figure 4 This is a long cycle diagram of the silicon negative electrode material with in-situ generated electrolyte additive obtained in Example 4. It can be seen that the sample has excellent cycle stability.

[0020] The above-described embodiments are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the protection scope of the present invention.

Claims

1. A method for preparing a silicon negative electrode material with an in-situ generated electrolyte additive, characterized in that: The following steps are involved: Mix Si, Super-P and Mg3N2 in an air-tight condition; The mixture is ball-milled under an inert gas atmosphere to obtain a silicon-based negative electrode material.

2. The method for preparing a silicon negative electrode material with in-situ generated electrolyte additive according to claim 1, characterized in that: The mass ratio of Si, Super-P and Mg3N2 is (30-90):(5-10):(5-60).

3. The method for preparing a silicon negative electrode material with in-situ generated electrolyte additive according to claim 1 or 2, characterized in that: The mixing specifically comprises the following steps: firstly, grinding Si and Super-P uniformly for 15-20 minutes, and then adding Mg3N2 and grinding uniformly for 15-20 minutes.

4. The method for preparing a silicon negative electrode material with in-situ generated electrolyte additive according to claim 1, characterized in that: The inert gas is argon, helium or nitrogen.

5. The method for preparing a silicon negative electrode material with in-situ generated electrolyte additive according to claim 1, characterized in that: The ball mill is a planetary ball mill.

6. The method for preparing a silicon negative electrode material with in-situ generated electrolyte additive according to claim 1 or 5, characterized in that: The ball-to-material ratio of the ball mill is 160:1, the ball mill revolution speed is 200 rpm, and the ball mill time is 30 minutes.

7. A silicon negative electrode material for in-situ generation of electrolyte additives, characterized in that: The silicon negative electrode material is composed of Si, Super-P and Mg3N2 in a mass ratio of (30-90):(5-10):(5-60), and the Super-P is coated on the surface of Si.

8. The silicon negative electrode material for in-situ generation of electrolyte additives according to claim 7, characterized in that: The Mg3N2 forms lithium nitride and magnesium in situ during the cycle to achieve lithium ion diffusion. At the same time, magnesium provides additional sites for the diffusion of lithium ions to build an ion conductive network.

Citation Information

Cited By

  • Silicon-based negative electrode material for sulfide solid-state lithium battery and application thereof