Inorganic sodium supplement and preparation method thereof, positive electrode material, positive electrode plate and sodium ion battery

Through the development of the inorganic sodium supplement Na4n-aLiaFe2n-bMbO5 and surface coating technology, the problem of sodium ion loss caused by interface layer compounds in sodium-ion batteries has been solved, high irreversible specific capacity and air stability have been achieved, and the sodium-ion battery has been significantly improved. electrochemical properties.

CN118763216APending Publication Date: 2024-10-11SOUTHWEST UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410752749.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In existing sodium-ion batteries, the interface layer compounds cause irreversible loss of sodium ions during the charge and discharge process, reducing the charge and discharge efficiency and energy density of the battery. In addition, inorganic sodium supplementation agents have problems such as low irreversible specific capacity and poor air stability. .

Method used

Develop an inorganic sodium supplement Na4n-aLiaFe2n-bMbO5. By adjusting its chemical composition and preparation method, adding the metal element M to increase the migration channel of sodium ions, and improving its air stability and conductive properties through surface coating technology.

Benefits of technology

The inorganic sodium supplementing agent has good sodium supplementing effect, high irreversible specific capacity and good air stability. It is suitable for sodium-ion batteries, significantly improves the electrochemical performance of the battery, and the preparation process is simple and easy to operate, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763216A_ABST
    Figure CN118763216A_ABST
Patent Text Reader

Abstract

The invention relates to an inorganic sodium supplementing agent and a preparation method thereof, a positive electrode material, a positive electrode plate and a sodium ion battery, and belongs to the technical field of sodium ion batteries. The inorganic sodium supplementing agent is prepared through a simple sol-gel-solid phase method, and the chemical formula of the inorganic sodium supplementing agent is Na4n-aLiaFe2n-bMbO5 (n is a positive integer smaller than 10, a is larger than 0 and smaller than 4n, and blt is larger than or equal to 0; m is any one or more of B, Mg, Al, K, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Mo or Sn). The inorganic sodium supplementing agent is excellent in sodium supplementing effect, high in irreversible specific capacity and stable to air. When the inorganic sodium supplement is subjected to surface coating, the air stability and the conductivity of the sodium supplement can be further improved. Due to the excellent performance of the sodium supplementing agent, the sodium supplementing agent has huge commercial application value in the field of sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and relates to an inorganic sodium supplement and a preparation method thereof, a positive electrode material, a positive electrode sheet and a sodium ion battery. Background Art

[0002] In electrochemical energy storage technology, lithium-ion batteries occupy the dominant position in the energy storage market due to their advantages of good safety performance and high specific capacity. However, due to the relative scarcity and uneven distribution of lithium resources in the earth's crust, their application is subject to certain restrictions.

[0003] As a homologous element of lithium, sodium has a high abundance, and sodium-ion batteries have excellent electrochemical comprehensive properties, so they are regarded as possible substitutes for lithium-ion batteries. Although the energy density of sodium-ion batteries is not as high as that of lithium-ion batteries, with the development and modification of sodium-ion battery cathode materials in recent years, the gap between the two has gradually narrowed. In a sodium-ion full battery, active sodium ions are released from the cathode and transferred to the cathode through the electrolyte, and the cathode loses sodium ions to form an interface film. It is well known that the cycle life of the battery is closely related to the stability of the interface. During the charge and discharge process, the interface layer compounds often affect the transmission of sodium ions. The SEl film formed by the first cycle of charging may cause irreversible loss of some sodium ions, thereby reducing the battery charge and discharge efficiency and affecting the energy density. To solve such problems, on the one hand, the material itself can be regulated and designed to promote its first efficiency and thus reduce the loss of active sodium ions; on the other hand, the electrolyte can be regulated to make the interface compound more stable. Among them, the regulation and design of the material itself, such as adding sodium supplements to the cathode material, is considered to be the most promising method.

[0004] Sodium supplement additives should meet the following requirements: (1) The oxidation potential of the additive should be lower than the operating potential of the whole battery, so as to ensure that active sodium ions are released within the operating voltage range of the whole battery; (2) The sodium ions released by the additive should be irreversible, that is, after the first charge, not much discharge capacity will be generated; (3) The additive needs to have a high charge specific capacity, and the decomposition products will not affect the positive electrode and have no adverse effects on the subsequent cycles of the whole battery.

[0005] The sodium supplement additives reported so far are mainly organic compounds. However, in addition to the release of sodium ions during the charging process, some of these sodium supplement additives are also accompanied by the generation of gas, which causes the internal gas pressure of the battery to increase, and in severe cases, it will affect the cycle life and safety performance of the battery. In contrast, inorganic materials have attracted much attention because they do not produce gas, but the inorganic sodium supplements reported so far have problems such as low irreversible specific capacity and poor air stability. Therefore, it is necessary to continue to develop inorganic sodium supplements with excellent performance for sodium-ion batteries. Summary of the invention

[0006] In view of this, one of the objects of the present invention is to provide an inorganic sodium supplement; the second object of the present invention is to provide a method for preparing an inorganic sodium supplement; the third object of the present invention is to provide a method for preparing a surface-coated inorganic sodium supplement; the fourth object of the present invention is to provide a surface-coated inorganic sodium supplement; the fifth object of the present invention is to provide a positive electrode material for a sodium ion battery; the sixth object of the present invention is to provide a positive electrode sheet for a sodium ion battery; the seventh object of the present invention is to provide a sodium ion battery.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] 1. An inorganic sodium supplement, wherein the chemical formula of the inorganic sodium supplement is Na 4n-a Li a Fe 2n-b M b O5, wherein n is a positive integer less than 10, 0<a<4n, 0≤b<2n, and M is any one or more of B, Mg, Al, K, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Mo or Sn.

[0009] 2. The preparation method of the inorganic sodium supplement is as follows:

[0010] (1) weighing compounds corresponding to the non-oxygen elements according to the stoichiometric ratio of the non-oxygen elements in the chemical formula of the inorganic sodium supplement, and then dissolving the compounds corresponding to the non-oxygen elements in deionized water to form a solution, adjusting the pH of the solution to 6 to 9, and stirring at 70 to 150° C. until gelation;

[0011] (2) The gel in step (1) is dried at 80-200° C. for 0.1-48 h, ground and sieved, and then placed in an inert atmosphere for reaction at 300-1200° C. for 5-120 h. After the reaction is completed, the gel is naturally cooled to room temperature.

[0012] 3. A method for preparing a surface-coated inorganic sodium supplement, the preparation method being as follows:

[0013] (1) weighing compounds corresponding to each non-oxygen element according to the stoichiometric ratio of each non-oxygen element in the chemical formula of the inorganic sodium supplement, then dissolving the compounds corresponding to each non-oxygen element in deionized water to form a solution, then adding a precursor of the coating to the solution, adjusting the pH of the solution to 6 to 9, and stirring at 70 to 150° C. until gelation;

[0014] The precursor of the coating is any one or more of acetylene black, Super P, Ketjen black, graphite, carbon nanotubes, graphene oxide, starch, ascorbic acid, polyvinyl pyrrolidone, tannic acid, polyethylene glycol, sucrose, glucose, polydopamine, dopamine, citric acid, phenolic resin, phosphate or aluminum isopropoxide;

[0015] (2) The gel in step (1) is dried at 80-200° C. for 0.1-48 h, ground and sieved, and then placed in an inert atmosphere for reaction at 300-1200° C. for 5-120 h. After the reaction is completed, the gel is naturally cooled to room temperature.

[0016] Preferably, the mass of the precursor of the coating in step (1) is 10% of the total mass of the compounds corresponding to the non-oxygen elements.

[0017] 4. The surface-coated inorganic sodium supplement prepared according to the preparation method.

[0018] 5. A positive electrode material for a sodium ion battery, comprising a positive electrode active material, a conductive agent and a binder, and also comprising any one or both of the inorganic sodium supplement or the surface-coated inorganic sodium supplement.

[0019] Preferably, the positive electrode active material includes any one or more of layered metal oxides, polyanionic compounds or Prussian blue compounds; the conductive agent includes any one or more of Ketjen black, acetylene black, Super P, single-walled carbon nanotubes or multi-walled carbon nanotubes; the binder includes any one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene butadiene rubber, styrene butadiene rubber, sodium carboxymethyl cellulose, polypropylene, polyethylene, polyacrylic acid, carboxymethyl cellulose, sodium alginate or gelatin; the mass of the inorganic sodium supplement is 0.2% to 30% of the mass of the positive electrode material for the sodium ion battery; the mass of the surface-coated inorganic sodium supplement is 0.2% to 30% of the mass of the positive electrode material for the sodium ion battery.

[0020] 6. A positive electrode sheet for a sodium ion battery, comprising the positive electrode material for a sodium ion battery.

[0021] 7. A sodium ion battery, comprising the positive electrode sheet for the sodium ion battery.

[0022] The beneficial effects of the present invention are as follows: the present invention provides an inorganic sodium supplement and a preparation method thereof, a positive electrode material, a positive electrode plate and a sodium ion battery. The chemical formula of the inorganic sodium supplement is Na 4n-a Li a Fe 2n-b M bO5 (wherein n is a positive integer less than 10, 0<a<4n, 0≤b<2n, and M is any one or more of B, Mg, Al, K, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Mo or Sn). The sodium supplement has a good sodium supplement effect, a high irreversible specific capacity and good air stability. When the metal element M is introduced, the migration channel of the sodium ions can be increased, the voltage of the sodium supplement can be reduced, and the irreversible specific capacity can be further improved. When the inorganic sodium supplement is surface coated, the air stability and conductivity of the sodium supplement can be further improved. The excellent performance of the sodium supplement in the present invention makes it extremely suitable for use in the field of sodium ion batteries. In addition, the preparation process of the sodium supplement in the present invention is simple and easy to operate, and is suitable for industrial production.

[0023] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0025] Figure 1 Na4Fe2O5 and the inorganic sodium supplement Na prepared in Example 1 3.8 Li 0.2 XRD pattern of Fe2O5;

[0026] Figure 2 The inorganic sodium supplement Na prepared in Example 1 3.8 Li 0.2 SEM image of Fe2O5;

[0027] Figure 3 The inorganic sodium supplement (Na 3.8 Li 0.2 EDS image of Fe2O5@C);

[0028] Figure 4 The inorganic sodium supplement (Na 3.8 Li 0.2 EDS graph of Fe2O5@PO). DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and the features in the embodiments can be combined with each other without conflict.

[0030] Example 1

[0031] An inorganic sodium supplement, the chemical formula of which is Na 3.8 Li 0.2 Fe2O5, its preparation method is as follows:

[0032] (1) According to the chemical formula Na 3.8 Li 0.2 The stoichiometric ratio of Na, Li and Fe in Fe2O5 was 3.8 mol NaOH, 0.2 mol LiOH and 1 mol Fe2O3, respectively, and then each compound was dissolved in 20 mL deionized water to form a solution, and the pH of the solution was adjusted to 9 with ammonia water and stirred at 80 °C until gel;

[0033] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 12 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 400° C. for 30 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0034] The inorganic sodium supplement Na prepared in Example 1 3.8 Li 0.2 Fe2O5 was subjected to X-ray powder diffraction test, and the experimental results are as follows Figure 1 As shown. Figure 1 It can be seen that the diffraction peak of the inorganic sodium supplement is basically consistent with the diffraction peak of Na4Fe2O5, and only some peak intensities will change, that is, the introduction of Li does not affect the overall peak structure of the material.

[0035] The inorganic sodium supplement Na prepared in Example 1 3.8 Li 0.2 Fe2O5 was observed for morphology. The experimental results are as follows Figure 2 As shown. Figure 2 It can be seen that the inorganic sodium supplement is mainly in the form of spheres and sticks.

[0036] Example 2

[0037] An inorganic sodium supplement, the chemical formula of the inorganic sodium supplement is Na3LiFe2O5, and the preparation method thereof is as follows:

[0038] (1) According to the stoichiometric ratio of Na, Li and Fe in the chemical formula Na3LiFe2O5, 3 mol NaOH, 1 mol LiOH and 2 mol FeCl3 were weighed respectively, and then each compound was dissolved in 25 mL deionized water to form a solution, and the pH of the solution was adjusted to 9 with ammonia water and then stirred at 80°C until gelation;

[0039] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 10 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 400° C. for 30 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0040] Example 3

[0041] An inorganic sodium supplement, the chemical formula of which is Na 3.8 Li 0.2 Fe 1.8 Mn 0.2 O5, the preparation method thereof is as follows:

[0042] (1) According to the chemical formula Na 3.8 Li 0.2 Fe 1.8 Mn 0.2 The stoichiometric ratio of Na, Li, Fe and Mn in O5 was 3.8 mol NaOH, 0.2 mol LiOH, 0.9 mol Fe2O3 and 0.1 mol Mn2O3, respectively. Each compound was then dissolved in 20 mL of deionized water to form a solution. The pH of the solution was adjusted to 8 with ammonia water and stirred at 70 °C until it gelled.

[0043] (2) The gel prepared in step (1) was placed in a 100° C. forced air drying oven for 6 h, and the dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 600° C. for 20 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0044] Example 4

[0045] An inorganic sodium supplement, the chemical formula of which is Na 3.8 Li 0.2 Fe 1.7 Al 0.3 O5, the preparation method thereof is as follows:

[0046] (1) According to the chemical formula Na3.8 Li 0.2 Fe 1.7 Al 0.3 The stoichiometric ratios of Na, Li, Fe and Al in O5 were 3.8 mol NaOH and 0.2 mol LiOH, 0.85 mol Fe2O3 and 0.15 mol Al2O3 were weighed respectively, and then each compound was dissolved in 30 mL deionized water to form a solution, and the pH of the solution was adjusted to 9 with ammonia water and stirred at 80 °C until gelation;

[0047] (2) The gel prepared in step (1) was placed in a 100° C. forced air drying oven and dried for 8 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 700° C. for 15 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0048] Example 5

[0049] An inorganic sodium supplement, the chemical formula of which is Na 3.5 Li 0.5 Fe 1.6 Ti 0.4 O5, the preparation method thereof is as follows:

[0050] (1) According to the chemical formula Na 3.5 Li 0.5 Fe 1.6 Ti 0.4 The stoichiometric ratio of Na, Li, Fe and Ti in O5 was 1.75 mol Na2CO3, 0.5 mol LiOH, 0.8 mol Fe2O3 and 0.4 mol TiO2, respectively. Each compound was then dissolved in 30 mL of deionized water to form a solution. The pH of the solution was adjusted to 9 with ammonia water and stirred at 100 °C until gelled;

[0051] (2) The gel prepared in step (1) was placed in a 100° C. forced air drying oven and dried for 24 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 550° C. for 40 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0052] Example 6

[0053] An inorganic sodium supplement, the chemical formula of which is Na 3.5 Li 0.5 Fe 0.5 Cu 1.5 O5, the preparation method thereof is as follows:

[0054] (1) According to the chemical formula Na 3.5 Li 0.5 Fe 0.5 Cu 1.5 The stoichiometric ratio of Na, Li, Fe and Cu in O5 was 1.75 mol Na2CO3 and 0.5 mol LiOH, 0.25 mol Fe2O3 and 1.5 mol CuO, respectively. Each compound was then dissolved in 40 mL of deionized water to form a solution. The pH of the solution was adjusted to 8.5 with aqueous ammonia and then stirred at 80 °C until gelled;

[0055] (2) The gel prepared in step (1) was placed in a 100° C. forced air drying oven and dried for 24 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 650° C. for 24 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0056] Example 7

[0057] An inorganic sodium supplement, the chemical formula of which is Na 3.5 Li 0.5 Fe 0.5 Ni 1.5 O5, the preparation method thereof is as follows:

[0058] (1) According to the chemical formula Na 3.5 Li 0.5 Fe 0.5 Ni 1.5 The stoichiometric ratio of Na, Li, Fe and Ni in O5 was 1.75 mol Na2CO3 and 0.5 mol LiOH, 0.25 mol Fe2O3 and 1.5 mol NiO, respectively. Each compound was then dissolved in 50 mL of deionized water to form a solution. The pH of the solution was adjusted to 8.5 with ammonia water and stirred at 80 °C until gelled;

[0059] (2) The gel prepared in step (1) is placed in a 90° C. forced air drying oven and dried for 20 h. The dried material is ground and sieved in sequence. After the treatment, it is transferred to a tubular furnace filled with argon and reacted at 750° C. for 20 h. After the reaction is completed, it is naturally cooled to room temperature and then stored in a glove box for later use.

[0060] Example 8

[0061] An inorganic sodium supplement, the chemical formula of which is Na 3.5 Li 0.5 Fe 0.8 Zn 1.2 O5, the preparation method thereof is as follows:

[0062] (1) According to the chemical formula Na 3.5 Li 0.5 Fe 0.8 Zn 1.2 The stoichiometric ratio of Na, Li, Fe and Zn in O5 was 1.75 mol Na2CO3 and 0.5 mol LiOH, 0.4 mol Fe2O3 and 1.2 mol ZnO, respectively. Each compound was then dissolved in 20 mL of deionized water to form a solution. The pH of the solution was adjusted to 9 with ammonia water and stirred at 80 °C until it gelled;

[0063] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 20 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 500° C. for 40 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for future use.

[0064] Example 9

[0065] An inorganic sodium supplement, the chemical formula of which is Na 3.5 Li 0.5 Fe 1.7 K 0.3 O5, the preparation method thereof is as follows:

[0066] (1) According to the chemical formula Na 3.5 Li 0.5 Fe 1.7 K 0.3 The stoichiometric ratios of Na, Li, Fe and K in O5 were 3.5 mol NaOH and 0.5 mol LiOH, 1.7 mol FeNO3 and 0.3 mol KNO3, respectively, and then each compound was dissolved in 20 mL deionized water to form a solution, and the pH of the solution was adjusted to 7.5 with ammonia water and stirred at 80 °C until gel;

[0067] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 10 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 700° C. for 30 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0068] Similarly, X-ray powder diffractometer and scanning electron microscope were used to characterize the inorganic sodium supplement prepared in Examples 2 to 9. The experimental results show that the diffraction peaks of the prepared materials are consistent with Na4Fe2O5, which indicates that the inorganic sodium supplement in Examples 2 to 9 was successfully synthesized.

[0069] Example 10

[0070] An inorganic sodium supplement with carbon coating on the surface (denoted as Na 3.8 Li 0.2 Fe2O5@C), the preparation method thereof is as follows:

[0071] (1) According to the chemical formula Na 3.8 Li 0.2 The stoichiometric ratio of Na, Li and Fe in Fe2O5 is as follows: 3.8 mol NaOH, 0.2 mol LiOH and 1 mol Fe2O3 are weighed respectively, and then each compound is dissolved in 20 mL deionized water to form a solution, and then glucose with a mass of 10% of the total mass of the above compounds is added to the solution, and ammonia water is added dropwise to adjust the pH of the solution to 9, and then stirred at 80°C until gel;

[0072] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 12 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 400° C. for 30 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0073] Embodiment 11

[0074] An inorganic sodium supplement with phosphate coating on the surface (denoted as Na 3.8 Li 0.2 Fe2O5@PO), the preparation method thereof is as follows:

[0075] (1) According to the chemical formula Na 3.8 Li 0.2 The stoichiometric ratio of Na, Li and Fe in Fe2O5 is as follows: 3.8 mol NaOH, 0.2 mol LiOH and 1 mol Fe2O3 are weighed respectively, and then each compound is dissolved in 20 mL deionized water to form a solution, and then lithium phosphate with a mass of 10% of the total mass of the above compounds is added to the solution, and ammonia water is added dropwise to adjust the pH of the solution to 9, and then stirred at 80°C until gel;

[0076] (2) The gel prepared in step (1) was placed in a forced air drying oven at 80° C. and dried for 12 h. The dried material was ground and sieved in sequence. After the treatment, it was transferred to a tubular furnace filled with argon and reacted at 400° C. for 30 h. After the reaction was completed, it was naturally cooled to room temperature and then stored in a glove box for later use.

[0077] Figure 3 The inorganic sodium supplement (Na 3.8 Li 0.2 Element distribution diagram of Fe2O5@C). Figure 3It can be clearly seen that the inorganic sodium supplement contains C element, which shows that carbon is successfully coated on Na 3.8 Li 0.2 The surface of Fe2O5. Figure 4 The inorganic sodium supplement (Na 3.8 Li 0.2 Element distribution diagram of Fe2O5@PO). Figure 4 It can be clearly seen that the inorganic sodium supplement contains P element, which shows that phosphate is successfully coated on Na 3.8 Li 0.2 The surface of Fe2O5.

[0078] Example 12

[0079] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 1 3.8 Li 0.2 Fe2O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0080] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.8 Li 0.2 Fe2O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then slice it after drying.

[0081] Example 13

[0082] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na3LiFe2O5 prepared in Example 2. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0083] Weigh Na and 2 / 3 Ni1 / 3 Mn 1 / 3 Ti 1 / 3 O2, Na3LiFe2O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then slice it after drying.

[0084] Embodiment 14

[0085] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 3 3.8 Li 0.2 Fe 1.8 Mn 0.2 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0086] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.8 Li 0.2 Fe 1.8 Mn 0.2 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0087] Embodiment 15

[0088] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 4 3.8 Li 0.2 Fe 1.7 Al 0.3 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0089] Weigh Na and 2 / 3 Ni1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.8 Li 0.2 Fe 1.7 Al 0.3 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0090] Example 16

[0091] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 5 3.5 Li 0.5 Fe 1.6 Ti 0.4 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0092] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.5 Li 0.5 Fe 1.6 Ti 0.4 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0093] Embodiment 17

[0094] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 6 3.5 Li 0.5 Fe 0.5 Cu 1.5 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0095] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.5 Li 0.5 Fe 0.5 Cu 1.5 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0096] Embodiment 18

[0097] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 7 3.5 Li 0.5 Fe 0.5 Ni 1.5 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0098] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.5 Li 0.5 Fe 0.5 Ni 1.5 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0099] Embodiment 19

[0100] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 8 3.5 Li 0.5 Fe 0.8 Zn1.2 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0101] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.5 Li 0.5 Fe 0.8 Zn 1.2 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0102] Embodiment 20

[0103] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and inorganic sodium supplement Na prepared in Example 9 3.5 Li 0.5 Fe 1.7 K 0.3 O5. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0104] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.5 Li 0.5 Fe 1.7 K 0.3 O5, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0105] Embodiment 21

[0106] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3O2, conductive agent KJ600, binder PVDF and the inorganic sodium supplement (Na 3.8 Li 0.2 Fe2O5@C). The specific preparation method of the corresponding positive electrode sheet is as follows:

[0107] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.8 Li 0.2 Fe2O5@C, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then slice it after drying.

[0108] Embodiment 22

[0109] A positive electrode material for a sodium ion battery, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, conductive agent KJ600, binder PVDF and the surface-coated phosphate inorganic sodium supplement (Na 3.8 Li 0.2 Fe2O5@PO). The specific preparation method of the corresponding positive electrode sheet is as follows:

[0110] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2、Na 3.8 Li 0.2 Fe2O5@PO, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then slice it after drying.

[0111] Comparative Example 1

[0112] A positive electrode material for a sodium ion battery that does not contain an inorganic sodium supplement, the positive electrode material comprising a positive electrode active material P2-type layered transition metal oxide Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3O2, conductive agent KJ600 and binder PVDF. The specific preparation method of the corresponding positive electrode sheet is as follows:

[0113] Weigh Na and 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2, PVDF and KJ600, then fully dissolve each substance in NMP to form a slurry, use a 200μm scraper to evenly coat the obtained slurry on the carbon-coated aluminum foil, then transfer it to a vacuum drying oven at 80℃ and dry it for 12h, and then cut it into slices after drying.

[0114] Performance Testing

[0115] The electrode sheets prepared in Examples 12 to 22 and Comparative Example 1 were used as positive electrodes, the metal sodium sheet was used as negative electrodes, the glass fiber was used as a separator, and 1M NaClO4+EC / PC (1:1, v / v) was used as an electrolyte. The button cells were assembled in a glove box filled with argon gas to prepare half cells. The button cell model was CR2032. The electrochemical performance of each half cell was tested at a current density of 20 mA / g in the voltage range of 2.5 to 4.5 V. The test results are shown in Table 1.

[0116] Table 1 Comparison of electrochemical performance of half-cells made with the positive electrode sheets in Examples 12 to 22 and Comparative Example 1

[0117]

[0118]

[0119] As can be seen from Table 1, compared with the half-cell made from the positive electrode sheet in Comparative Example 1, the discharge specific capacity of the half-cells made from the positive electrode sheets in Examples 12 to 22 did not change much, indicating that the inorganic sodium supplement contained in each positive electrode sheet or the inorganic sodium supplement coated on the surface decomposed after the first cycle of charging, but was irreversible during the discharge process, thereby not causing additional discharge specific capacity. From the perspective of the capacity retention rate of the long cycle, compared with the half-cell made from the positive electrode sheet in Comparative Example 1, the capacity retention rate of the half-cells made from the positive electrode sheets in Examples 12 to 22 was higher, indicating that the inorganic sodium supplement contained in each positive electrode sheet or the inorganic sodium supplement coated on the surface played a role in the first cycle of sodium supplementation, and its residual byproducts did not affect the subsequent performance of the positive electrode. The above results show that when the inorganic sodium supplement or the inorganic sodium supplement coated on the surface in the present invention is applied to the field of sodium supplementation, it has excellent sodium supplementation effect, high irreversible specific capacity, and good air stability, thus having great commercial value.

[0120] In summary, the present invention provides an inorganic sodium supplement and a preparation method thereof, a positive electrode material, a positive electrode plate and a sodium ion battery. The sodium supplement has a high irreversible specific capacity and good air stability. When used in the positive electrode material of a sodium ion battery, the electrochemical performance of the battery can be significantly improved. In addition, the sodium supplement in the present invention has no special restrictions on the current collector, active material, binder, conductive additive and even the electrolyte and diaphragm of the sodium ion battery in the positive electrode material, and has a wide range of applicability.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. An inorganic sodium supplement, characterized in that: The chemical formula of the inorganic sodium supplement is Na 4n-a Li a Fe 2n-b M b O5, wherein n is a positive integer less than 10, 0<a<4n, 0≤b<2n, and M is any one or more of B, Mg, Al, K, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Mo or Sn.

2. The method for preparing the inorganic sodium supplement according to claim 1, characterized in that: The preparation method is as follows: (1) weighing compounds corresponding to the non-oxygen elements according to the stoichiometric ratio of the non-oxygen elements in the chemical formula of the inorganic sodium supplement, and then dissolving the compounds corresponding to the non-oxygen elements in deionized water to form a solution, adjusting the pH of the solution to 6 to 9, and stirring at 70 to 150° C. until gelation; (2) The gel in step (1) is dried at 80-200° C. for 0.1-48 h, ground and sieved, and then placed in an inert atmosphere for reaction at 300-1200° C. for 5-120 h. After the reaction is completed, the gel is naturally cooled to room temperature.

3. A method for preparing a surface-coated inorganic sodium supplement, characterized in that: The preparation method is as follows: (1) Weighing compounds corresponding to the non-oxygen elements according to the stoichiometric ratio of the non-oxygen elements in the chemical formula of the inorganic sodium supplement according to claim 1, and then dissolving the compounds corresponding to the non-oxygen elements in deionized water to form a solution, then adding a precursor of the coating to the solution, adjusting the pH of the solution to 6-9, and stirring at 70-150° C. until gelation; The precursor of the coating is any one or more of acetylene black, Super P, Ketjen black, graphite, carbon nanotubes, graphene oxide, starch, ascorbic acid, polyvinyl pyrrolidone, tannic acid, polyethylene glycol, sucrose, glucose, polydopamine, dopamine, citric acid, phenolic resin, phosphate or aluminum isopropoxide; (2) The gel in step (1) is dried at 80-200° C. for 0.1-48 h, ground and sieved, and then placed in an inert atmosphere for reaction at 300-1200° C. for 5-120 h. After the reaction is completed, the gel is naturally cooled to room temperature.

4. The preparation method according to claim 3, characterized in that: The mass of the precursor of the coating in step (1) is 10% of the total mass of the compounds corresponding to the non-oxygen elements.

5. The surface-coated inorganic sodium supplement prepared according to the preparation method according to any one of claims 3 or 4.

6. A positive electrode material for a sodium ion battery, comprising a positive electrode active material, a conductive agent and a binder, characterized in that: It also includes any one or both of the inorganic sodium supplement according to claim 1 or the surface-coated inorganic sodium supplement according to claim 5.

7. The positive electrode material for sodium ion battery according to claim 6, characterized in that: The positive electrode active material includes any one or more of layered metal oxides, polyanionic compounds or Prussian blue compounds; the conductive agent includes any one or more of Ketjen black, acetylene black, Super P, single-walled carbon nanotubes or multi-walled carbon nanotubes; the binder includes any one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene butadiene rubber, styrene butadiene rubber, sodium carboxymethyl cellulose, polypropylene, polyethylene, polyacrylic acid, carboxymethyl cellulose, sodium alginate or gelatin; the mass of the inorganic sodium supplement is 0.2% to 30% of the mass of the positive electrode material for the sodium ion battery; the mass of the surface-coated inorganic sodium supplement is 0.2% to 30% of the mass of the positive electrode material for the sodium ion battery.

8. A positive electrode sheet for a sodium ion battery, characterized in that: The positive electrode sheet for a sodium ion battery comprises the positive electrode material for a sodium ion battery according to any one of claims 6 or 7.

9. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sheet for the sodium ion battery according to claim 8.

Citation Information

Cited By

  • Needle-shaped sodium zirconium phosphate sodium supplement as well as preparation method and application thereof

    CN120109196A