Battery packaging film structure and preparation method and application thereof

By adopting a combined structure of a high-density interconnected circuit layer and a sensing film layer in a lithium-ion battery, the problems of inaccurate battery internal state monitoring and increased battery weight in the existing technology are solved, and real-time monitoring of the internal and external environment of the battery is achieved. , improving the safety and service life of the battery.

CN118763329AActive Publication Date: 2024-10-11TIANFU JIANGXI LAB
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202411237016.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-10-11
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing lithium-ion battery monitoring methods cannot effectively monitor the internal status of the battery, and internally implanted sensors increase the weight and structural complexity of the battery, affecting performance and safety.

Method used

It adopts a combined structure of high-density interconnected circuit layer and sensing film layer, realizes electrical connection and signal transmission through multi-layer structure and vertical via holes, integrates the sensing function into the battery packaging film, and monitors the internal and external environment of the battery in real time.

Benefits of technology

It improves battery detection accuracy and reliability, reduces battery weight and structural complexity, enhances battery safety and service life, and enables real-time monitoring and packaging protection of battery health status.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763329A_ABST
    Figure CN118763329A_ABST
Patent Text Reader

Abstract

The invention discloses a battery packaging film structure and a preparation method and application thereof, and relates to the technical field of lithium ion batteries, the battery packaging film structure comprises a high-density interconnection circuit layer and a sensing film layer, and the high-density interconnection circuit layer is located above the sensing film layer; the high-density interconnection circuit layers are divided by insulating media, and electrical connection between the upper layer and the lower layer is achieved through vertical via holes. The high-density interconnection circuit and the pressure sensing film layer are integrated together, real-time monitoring of the health state of the battery and packaging protection of the battery are achieved, the structure is simplified through the integrated design, and the reliability and stability of the system are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a battery packaging film structure and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in electronic devices, electric vehicles and energy storage systems due to their high energy density, long life and low self-discharge rate. However, as the use time increases, the performance of lithium-ion batteries will gradually decline, and even safety issues such as thermal runaway may occur. In order to ensure the performance and safety of lithium batteries, it is particularly important to monitor their health status (including parameters such as temperature, pressure, current, voltage, etc.) in real time.

[0003] Traditional battery monitoring methods mainly include the following: 1. Surface-mounted sensors have the following advantages: relatively mature technology, easy installation, and low cost. Their disadvantages are: they can only monitor the temperature and pressure on the surface of the battery, and cannot obtain the real data inside the battery. Therefore, the monitoring accuracy and reliability are limited, and they cannot effectively warn of potential safety hazards inside the battery.

[0004] 2. Internally implanted sensors have the advantages of being able to directly monitor key parameters such as temperature and pressure inside the battery with high data accuracy. The disadvantages are that a complex electrical signal extraction path needs to be designed, which increases the structural complexity of the battery. In addition, internally implanted sensors increase the weight of the battery, reduce the specific energy of the battery, and may affect the mechanical strength and overall performance of the battery.

[0005] Therefore, there is an urgent need for a new battery packaging film structure that can ensure detection accuracy without increasing the weight and structural complexity of the battery, thereby effectively solving the above problems. Summary of the invention

[0006] Based on the problems of low monitoring accuracy and reliability and heavy battery weight in current battery detection structures, the purpose of the present invention is to provide a battery packaging film structure and its preparation method and application, which can realize real-time monitoring of the internal state and external environment of the battery, improve the detection accuracy and reliability, make the battery lighter, and provide effective packaging protection.

[0007] The present invention is achieved through the following technical solutions: In the first aspect, the present application provides a battery packaging film structure, including a high-density interconnection circuit layer and a sensor film layer, wherein the high-density interconnection circuit layer is located above the sensor film layer; the high-density interconnection circuit layer has multiple layers, each layer is separated by an insulating medium, and the electrical connection between the upper and lower layers is achieved through vertical conductive holes.

[0008] Furthermore, the surface of the high-density interconnection circuit layer is covered with a polyimide protective film.

[0009] Furthermore, the method for preparing the high-density interconnect circuit layer comprises the following steps: Prepare the substrate: Select a polyimide film as the substrate; the thickness of the polyimide is 20 μm to 30 μm, preferably 25 μm. Specifically, cut the polyimide (PI) film into a suitable size and bake it at a temperature of 80°C to 100°C (preferably 90°C) for 20 min to 40 min (preferably 30 min) to remove moisture.

[0010] Photolithography and electroplating: The circuit pattern is defined by photolithography, and then copper is deposited by electroplating to form conductive lines; The photolithography process is specifically as follows: 1. Coating photoresist: Evenly coat a 2μm thick layer of photoresist on the PI film at a rotation speed of 2500rpm~3500rpm (preferably 3000rpm) for 20s~40s (preferably 30s).

[0011] 2. Baking: Bake the photoresist at a temperature of 80°C to 100°C (preferably 90°C) for 5 min to 15 min (preferably 10 min).

[0012] 3. Exposure: Use UV exposure equipment to expose 80mJ / cm through the mask 2 ~120mJ / cm 2 (Preferably 100Mj / cm 2 ).

[0013] 4. Development: Develop the exposed photoresist in developer (AZ726) for 50s~70s (preferably 60s), rinse and dry.

[0014] Among them, the electroplating process is specifically as follows: Copper layer deposition: electroplating is performed on the developed PI film. The electroplating solution is copper sulfate solution with a current density of 8 mA / cm 2 ~12mA / cm 2 (Preferably 10 mA / cm 2 ), the time is 8min~12min (preferably 10min), and a 10μm thick copper layer is formed.

[0015] Stacking and vertical vias: Coating a polyimide dielectric layer on each layer of circuits, then opening vertical vias, and then depositing copper to form upper and lower layer connections; repeating this process until the desired multi-layer structure is achieved; The specific process is: 1. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 1500 rpm to 2500 rpm (preferably 2000 rpm) for 20 s to 40 s (preferably 30 s).

[0016] 2. Drilling: Use laser drilling equipment to drill vertical through holes (Via) on the dielectric layer with a hole diameter of 40μm~60μm (preferably 50μm).

[0017] 3. Deposit copper for the second time: Repeat the photolithography and electroplating processes to form a second layer of copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0018] 4. Repeat the above steps until the desired multi-layer structure (e.g., 3 layers of high-density interconnect circuit layers) is achieved.

[0019] Packaging and protection: A polyimide protective film is covered on the surface of the multi-layer high-density interconnected circuit layer structure.

[0020] Specifically: a 5 μm thick polyimide (PI) protective film is covered on the surface of the multi-layer high-density interconnection circuit layer structure, the rotation speed is 1500rpm~2500rpm (preferably 2000rpm), the time is 20s~40s (preferably 30s), to ensure uniform coverage.

[0021] Furthermore, the method for preparing the sensing film comprises the following steps: Solution preparation: prepare the raw materials required for preparation into a solution; Specifically, PVDF powder is dissolved in dimethylacetamide (DMAc) solvent to prepare a solution of 8wt% to 12wt% (preferably 10wt%).

[0022] Solution casting: The prepared solution is evenly coated on a glass substrate and then dried to form a sensing film; Specifically, the PVDF solution is evenly coated on the glass substrate at a rotation speed of 800 rpm to 1200 rpm (preferably 1000 rpm) for 50 s to 70 s (preferably 60 s). The solution is baked at a temperature of 50°C to 70°C (preferably 60°C) for 45 min to 75 min (preferably 60 min) to form a uniform PVDF film with a thickness of 50 μm.

[0023] Polarization treatment: The sensing film is placed in an electric field for polarization treatment. The electric field strength is 0.8kV / mm~1.2kV / mm (preferably 1kV / mm) and the time is 20min~40min (preferably 30min). The piezoelectric properties of the sensing film are enhanced by polarization treatment.

[0024] In a second aspect, the present application provides a method for preparing a battery packaging film structure, comprising the following steps: Prepare the substrate: Select polyimide film as the substrate; Photolithography and electroplating: The circuit pattern is defined by photolithography, and then the copper layer is deposited by electroplating to form a conductive line; Stacking and vertical vias: Coating a polyimide dielectric layer on each layer of circuit (wherein the thickness of the polyimide dielectric layer is 3μm~7μm, preferably 5μm), then opening vertical vias, and then depositing copper to form upper and lower layer connections; repeating this process until the desired multi-layer structure is achieved; Packaging and protection: Cover the surface of the multi-layer high-density interconnected circuit layer structure with a polyimide protective film; Solution preparation: prepare the raw materials required for preparation into a solution; Solution casting: evenly coating the prepared solution on a glass substrate, and then drying to form a sensing film, wherein the sensing film comprises a polyvinylidene fluoride (PVDF) film with a thickness of 40 μm to 60 μm, preferably 50 μm; Polarization treatment: Place the sensing film in an electric field for polarization treatment; Assembly: stacking the prepared multi-layer high-density interconnection circuit layer and the sensor film, ensuring that the multi-layer high-density interconnection circuit layer is on the top and the sensor film is on the bottom, and using an adhesive to bond the multi-layer high-density interconnection circuit layer and the sensor film to ensure a close fit; Packaging: Heat sealing is used to ensure that the edges of the packaging film are tightly sealed. Ethylene-vinyl acetate copolymer (EVA) glue is used as the packaging glue.

[0025] The temperature during heat sealing is 140° C. to 160° C. (preferably 150° C.), the time is 3 s to 7 s (preferably 5 s), and the pressure is 0.4 MPa to 0.6 MPa (preferably 0.5 MPa).

[0026] Furthermore, the polyimide substrate for preparing the multi-layer high-density interconnection circuit layer is baked at a temperature of 80° C. to 100° C. to remove moisture before photolithography.

[0027] Furthermore, the thickness of the copper layer is 8 μm to 12 μm.

[0028] Furthermore, the aperture of the vertical via hole is 40µm ~ 60µm.

[0029] Furthermore, the solution for preparing the sensing membrane is a solution of 8 wt% to 12 wt% formed by dissolving polyvinylidene fluoride in dimethylacetamide solvent.

[0030] In a third aspect, the present application provides a lithium battery, comprising the battery packaging film structure described above or the battery packaging film structure prepared by the above preparation method.

[0031] When installing a lithium battery, the prepared packaging film is attached to the surface of the battery to ensure that the high-density interconnection circuit layer is connected to the sensor inside the battery cell, and the outer layer of the sensor film is exposed to the external environment.

[0032] Among them, the high-density interconnect circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external monitoring equipment through vertical conductive holes.

[0033] The sensing membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring device through the high-density interconnection circuit layer, realizing real-time monitoring of the battery's external environment.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The high-density interconnection circuit layer of the present invention adopts a clever combination of a multi-layer structure and vertical vias to achieve high-density signal transmission and reliable electrical connection.

[0035] (2) The present invention adopts a combination of a high-density interconnected circuit layer and a pressure sensing film layer, which not only realizes the efficient transmission of the sensing signal inside the battery, but also effectively isolates the influence of the external environment on the battery through its multi-layer structure, thereby improving the safety and service life of the battery.

[0036] (3) The present invention integrates a high-density interconnect circuit with a pressure sensing film layer to achieve real-time monitoring of the battery health status and packaging protection of the battery. This integrated design not only simplifies the structure but also improves the reliability and stability of the system.

[0037] (4) The high-density interconnection circuit layer of the present invention adopts a multi-layer structure and a vertical conductive hole design, which can efficiently transmit the temperature, pressure and other sensor signals inside the battery cell. These signals are transmitted to the external monitoring equipment through the high-density interconnection circuit layer, realizing real-time monitoring of the internal state of the battery.

[0038] (5) The high-density interconnection circuit layer of the present invention can effectively isolate the influence of external water vapor and oxygen on the battery through a multi-layer high-density interconnection structure, prevent the internal electrolyte from degrading and the motor material from oxidizing, thereby extending the service life of the battery.

[0039] (6) The sensing film layer of the present invention utilizes its excellent piezoelectric properties to sensitively respond to external pressure changes and monitor the external environment of the battery in real time. This precise pressure monitoring capability helps to discover and prevent potential safety problems of the battery at an early stage.

[0040] (7) The present invention optimizes the layout of the high-density interconnection structure layer and the pressure sensing film layer, so that the packaging film can both conduct electrical signals and provide mechanical protection. At the same time, the multi-layer high-density interconnection structure layer effectively blocks the influence of water and oxygen on the battery, thereby improving the overall safety and reliability of the battery.

[0041] (8) Compared with the traditional method of internally implanting sensors, the present invention maintains the high energy density of the battery without increasing the weight of the battery. By integrating the sensing and protection functions into the packaging film, the complex internal structure design is avoided, and the manufacturing cost and difficulty are reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings: Figure 1 It is a schematic diagram of the structure of the encapsulation film in the present invention; Figure 2 This is a diagram showing the sealing performance test results in Example 1 of the present invention; Figure 3 This is a diagram showing the signal transmission performance test results in Example 1 of the present invention; Figure 4 This is a diagram showing the sealing performance test results in Example 2 of the present invention; Figure 5 This is a diagram showing the signal transmission performance test results in Example 2 of the present invention; Figure 6 This is a diagram showing the sealing performance test results in Example 3 of the present invention; Figure 7 This is a diagram showing the signal transmission performance test results in Example 3 of the present invention; Figure 8 This is a diagram showing the sealing performance test results in Example 4 of the present invention; Fig. 9 This is a diagram showing the signal transmission performance test results in Example 4 of the present invention; Fig.10 This is a diagram showing the sealing performance test results in Example 5 of the present invention; Fig.11 This is a diagram of the signal transmission performance test results in Example 5 of the present invention. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0044] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] This embodiment provides a method for preparing a battery sealing film structure, and the specific steps are as follows: S1. Material preparation S1-1, base material: polyimide (PI) film, thickness: 25 μm.

[0047] S1-2, conductive material: copper (Cu) film, thickness: 10μm.

[0048] S1-3, Insulation material: polyimide (PI) coating, thickness: 5μm.

[0049] S1-4, Sensing membrane material: polyvinylidene fluoride (PVDF) film, thickness: 50μm.

[0050] S1-5, Packaging glue: ethylene-vinyl acetate copolymer (EVA) glue.

[0051] S2. Fabrication of high-density interconnection circuit layer S2-1. Substrate preparation: Cut the polyimide (PI) film into a suitable size and bake it at 90°C for 30 minutes to remove moisture.

[0052] S2-2. Photoresist coating: evenly coat a 2 μm thick layer of photoresist (AZ5214) on the PI film at a rotation speed of 3000 rpm for 30 seconds.

[0053] S2-3, baking: bake the photoresist at 90°C for 10 minutes.

[0054] S2-4, Exposure: Use UV exposure equipment, expose through the mask plate 100mJ / cm 2 .

[0055] S2-5, Development: Develop the exposed photoresist in developer (AZ726) for 60 seconds, rinse and dry.

[0056] S2-6, depositing copper layer: electroplating was performed on the developed PI film, the electroplating solution was copper sulfate solution, and the current density was 10 mA / cm 2 , time 10 minutes, forming a 10μm thick copper layer.

[0057] S2-7. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 2000 rpm for 30 seconds.

[0058] S2-8, Drilling: Use laser drilling equipment to drill vertical vias (Via) on the dielectric layer with a hole diameter of 50μm.

[0059] S2-9, deposit the second layer of copper: repeat the photolithography and electroplating processes to form a second layer of 10μm thick copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0060] S2-10, repeat the above steps until the desired multi-layer structure is achieved.

[0061] S2-11. Cover the surface of the multi-layer high-density interconnection circuit layer with a 5μm thick polyimide (PI) protective film at a speed of 2000rpm for 30s to ensure uniform coverage.

[0062] S3. Preparation of PVDF pressure sensing membrane S3-1. Solution preparation: Dissolve PVDF powder in dimethylacetamide (DMAc) solvent to prepare a 10 wt% solution.

[0063] S3-2, solution casting: the PVDF solution was evenly coated on the glass substrate at a rotation speed of 1000 rpm for 60 seconds.

[0064] S3-3. Drying: Bake at 60°C for 1 hour to form a uniform 50 μm thick PVDF film.

[0065] S3-4. Polarization treatment: The PVDF film is placed in an electric field for polarization treatment with an electric field strength of 1 kV / mm for 30 minutes to enhance its piezoelectric properties.

[0066] S4. Assemble the packaging film S4-1. Stack the prepared multi-layer high-density interconnection circuit layer and the PVDF pressure sensing film layer, ensuring that the multi-layer high-density interconnection circuit layer is on the upper side and the PVDF pressure sensing film layer is on the lower side.

[0067] S4-2, use EVA glue to bond the two layers to ensure close fit; heat seal at 150°C for 5 seconds and at a pressure of 0.5 MPa to ensure that the edges of the packaging film are tightly sealed to prevent air and moisture from entering, and obtain a packaging film, the structure of which is as follows: Figure 1 shown.

[0068] The prepared packaging film is applied to the packaging of lithium batteries, and the packaging film is adhered to the surface of the battery to ensure that the multi-layer high-density interconnected circuit layer is connected to the sensor inside the battery cell, and the outer layer of the PVDF film is exposed to the external environment.

[0069] Among them, the multi-layer high-density interconnected circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external detection equipment through vertical conductive holes.

[0070] The PVDF membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring equipment through multiple layers of high-density interconnected circuit layers, thus achieving real-time monitoring of the battery's external environment.

[0071] The performance of a lithium battery prepared using the packaging film prepared in this embodiment was tested.

[0072] The packaged batteries are placed in a high temperature and high humidity environment for testing to verify the sealing performance, signal transmission performance and environmental isolation capabilities of the packaging film.

[0073] 1. Sealing performance test Testing conditions: High temperature environment: 85℃, for 72 hours.

[0074] High humidity environment: 85% relative humidity (RH) for 72 hours.

[0075] Cycle environment: high and low temperature cycle test, temperature range: -20℃~85℃, each cycle is 24 hours, a total of 10 cycles, the test results are as follows Figure 2 shown.

[0076] The helium leak detection data is: Initial helium leakage rate: 1×10 -7 cc / s ; After high temperature environment: 1.2×10 -7 cc / s ; After high humidity environment: 1.1×10 -7 cc / s ; After cycle environment: 1.3×10 -7 cc / s .

[0077] 2. Signal transmission performance test, test results such as Figure 3 shown.

[0078] Testing conditions: Normal working environment: 25℃, for 24 hours.

[0079] High temperature environment: 85℃, for 24 hours.

[0080] Low temperature environment: -20℃, for 24 hours.

[0081] Resistance test data: 25℃:0.1Ω 85℃: 0.12Ω -20℃:0.15Ω.

[0082] 3. Environmental isolation capability test Testing conditions: High humidity environment: 85% relative humidity (RH) for 72 hours.

[0083] Salt spray environment: Salt spray test, 5% sodium chloride solution, for 48 hours.

[0084] Weight change test data: Before high humidity environment: 200.0mg After high humidity environment: 202.0mg Before salt spray environment: 200.0mg After salt spray environment: 203.0mg.

[0085] Example 2

[0086] This embodiment provides a method for preparing a battery sealing film structure. The difference from Embodiment 1 is that the thickness of the copper layer in this embodiment is 8 μm. The other steps are the same as Embodiment 1. The specific steps are as follows: S1. Material preparation S1-1, base material: polyimide (PI) film, thickness: 25 μm.

[0087] S1-2, conductive material: copper (Cu) film, thickness: 10μm.

[0088] S1-3, Insulation material: polyimide (PI) coating, thickness: 5μm.

[0089] S1-4, Sensing membrane material: polyvinylidene fluoride (PVDF) film, thickness: 50μm.

[0090] S1-5, Packaging glue: ethylene-vinyl acetate copolymer (EVA) glue.

[0091] S2. Fabrication of high-density interconnection circuit layer S2-1. Substrate preparation: Cut the polyimide (PI) film into a suitable size and bake it at 90°C for 30 minutes to remove moisture.

[0092] S2-2. Photoresist coating: evenly coat a 2 μm thick layer of photoresist (AZ5214) on the PI film at a rotation speed of 3000 rpm for 30 seconds.

[0093] S2-3, baking: bake the photoresist at 90°C for 10 minutes.

[0094] S2-4, Exposure: Use UV exposure equipment, expose through the mask plate 100mJ / cm 2 .

[0095] S2-5, Development: Develop the exposed photoresist in developer (AZ726) for 60 seconds, rinse and dry.

[0096] S2-6, depositing copper layer: electroplating was performed on the developed PI film, the electroplating solution was copper sulfate solution, and the current density was 10 mA / cm 2 , time 10 minutes, forming a copper layer with a thickness of 8μm.

[0097] S2-7. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 2000 rpm for 30 seconds.

[0098] S2-8, Drilling: Use laser drilling equipment to drill vertical vias (Via) on the dielectric layer with a hole diameter of 50μm.

[0099] S2-9, deposit the second layer of copper: repeat the photolithography and electroplating processes to form a second layer of 8μm thick copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0100] S2-10, repeat the above steps until the desired multi-layer structure is achieved.

[0101] S2-11. Cover the surface of the multi-layer high-density interconnection circuit layer with a 5μm thick polyimide (PI) protective film at a speed of 2000rpm for 30s to ensure uniform coverage.

[0102] S3. Preparation of PVDF pressure sensing membrane S3-1. Solution preparation: Dissolve PVDF powder in dimethylacetamide (DMAc) solvent to prepare a 10 wt% solution.

[0103] S3-2, solution casting: the PVDF solution was evenly coated on the glass substrate at a rotation speed of 1000 rpm for 60 seconds.

[0104] S3-3. Drying: Bake at 60°C for 1 hour to form a uniform 50 μm thick PVDF film.

[0105] S3-4. Polarization treatment: The PVDF film is placed in an electric field for polarization treatment with an electric field strength of 1 kV / mm for 30 minutes to enhance its piezoelectric properties.

[0106] S4. Assemble the packaging film S4-1. Stack the prepared multi-layer high-density interconnection circuit layer and the PVDF pressure sensing film layer, ensuring that the multi-layer high-density interconnection circuit layer is on the upper side and the PVDF pressure sensing film layer is on the lower side.

[0107] S4-2, use EVA glue to bond the two layers to ensure a close fit; heat seal at 150°C for 5 seconds and a pressure of 0.5 MPa to ensure that the edges of the packaging film are tightly sealed to prevent air and moisture from entering, and obtain the packaging film. The prepared packaging film is applied to the packaging of lithium batteries, and the packaging film is adhered to the surface of the battery to ensure that the multi-layer high-density interconnected circuit layer is connected to the sensor inside the battery cell, and the outer layer of the PVDF film is exposed to the external environment.

[0108] Among them, the multi-layer high-density interconnected circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external detection equipment through vertical conductive holes.

[0109] The PVDF membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring equipment through multiple layers of high-density interconnected circuit layers, thus achieving real-time monitoring of the battery's external environment.

[0110] The performance of a lithium battery prepared using the packaging film prepared in this embodiment was tested.

[0111] The packaged batteries are placed in a high temperature and high humidity environment for testing to verify the sealing performance, signal transmission performance and environmental isolation capabilities of the packaging film.

[0112] 1. Sealing performance test Testing conditions: High temperature environment: 85℃, for 72 hours.

[0113] High humidity environment: 85% relative humidity (RH) for 72 hours.

[0114] Cycle environment: high and low temperature cycle test, temperature range: -20℃~85℃, each cycle is 24 hours, a total of 10 cycles, the test results are as follows Figure 4 shown.

[0115] The helium leak detection data is: Initial helium leakage rate: 1×10 -7 cc / s ; After high temperature environment: 1.3×10 -7 cc / s ; After high humidity environment: 1.2×10 -7 cc / s ; After cycle environment: 1.4×10 -7 cc / s .

[0116] 2. Signal transmission performance test, test results such as Figure 5 shown.

[0117] Testing conditions: Normal working environment: 25℃, for 24 hours.

[0118] High temperature environment: 85℃, for 24 hours.

[0119] Low temperature environment: -20℃, for 24 hours.

[0120] Resistance test data: 25℃: 0.12Ω 85℃: 0.14Ω -20℃:0.17Ω.

[0121] 3. Environmental isolation capability test Testing conditions: High humidity environment: 85% relative humidity (RH) for 72 hours.

[0122] Salt spray environment: Salt spray test, 5% sodium chloride solution, for 48 hours.

[0123] Weight change test data: Before high humidity environment: 200.0mg After high humidity environment: 202.0mg Before salt spray environment: 200.0mg After salt spray environment: 202.5mg.

[0124] Example 3

[0125] This embodiment provides a method for preparing a battery sealing film structure. The difference from Embodiment 1 is that the thickness of the copper layer in this embodiment is 12 μm. The other steps are the same as Embodiment 1. The specific steps are as follows: S1. Material preparation S1-1, base material: polyimide (PI) film, thickness: 25 μm.

[0126] S1-2, conductive material: copper (Cu) film, thickness: 10μm.

[0127] S1-3, Insulation material: polyimide (PI) coating, thickness: 5μm.

[0128] S1-4, Sensing membrane material: polyvinylidene fluoride (PVDF) film, thickness: 50μm.

[0129] S1-5, Packaging glue: ethylene-vinyl acetate copolymer (EVA) glue.

[0130] S2. Fabrication of high-density interconnection circuit layer S2-1. Substrate preparation: Cut the polyimide (PI) film into a suitable size and bake it at 90°C for 30 minutes to remove moisture.

[0131] S2-2. Photoresist coating: evenly coat a 2 μm thick layer of photoresist (AZ5214) on the PI film at a rotation speed of 3000 rpm for 30 seconds.

[0132] S2-3, baking: bake the photoresist at 90°C for 10 minutes.

[0133] S2-4, Exposure: Use UV exposure equipment, expose through the mask plate 100mJ / cm 2 .

[0134] S2-5, Development: Develop the exposed photoresist in developer (AZ726) for 60 seconds, rinse and dry.

[0135] S2-6, depositing copper layer: electroplating was performed on the developed PI film, the electroplating solution was copper sulfate solution, and the current density was 10 mA / cm 2 , time 10 minutes, forming a 12μm thick copper layer.

[0136] S2-7. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 2000 rpm for 30 seconds.

[0137] S2-8, Drilling: Use laser drilling equipment to drill vertical vias (Via) on the dielectric layer with a hole diameter of 50μm.

[0138] S2-9, deposit the second layer of copper: repeat the photolithography and electroplating processes to form a second layer of 12μm thick copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0139] S2-10, repeat the above steps until the desired multi-layer structure is achieved.

[0140] S2-11. Cover the surface of the multi-layer high-density interconnection circuit layer with a 5μm thick polyimide (PI) protective film at a speed of 2000rpm for 30s to ensure uniform coverage.

[0141] S3. Preparation of PVDF pressure sensing membrane S3-1. Solution preparation: Dissolve PVDF powder in dimethylacetamide (DMAc) solvent to prepare a 10 wt% solution.

[0142] S3-2, solution casting: the PVDF solution was evenly coated on the glass substrate at a rotation speed of 1000 rpm for 60 seconds.

[0143] S3-3. Drying: Bake at 60°C for 1 hour to form a uniform 50 μm thick PVDF film.

[0144] S3-4. Polarization treatment: The PVDF film is placed in an electric field for polarization treatment with an electric field strength of 1 kV / mm for 30 minutes to enhance its piezoelectric properties.

[0145] S4. Assemble the packaging film S4-1. Stack the prepared multi-layer high-density interconnection circuit layer and the PVDF pressure sensing film layer, ensuring that the multi-layer high-density interconnection circuit layer is on the upper side and the PVDF pressure sensing film layer is on the lower side.

[0146] S4-2, use EVA glue to bond the two layers to ensure a close fit; heat seal at 150°C for 5 seconds and a pressure of 0.5 MPa to ensure that the edges of the packaging film are tightly sealed to prevent air and moisture from entering, and obtain the packaging film. The prepared packaging film is applied to the packaging of lithium batteries, and the packaging film is adhered to the surface of the battery to ensure that the multi-layer high-density interconnected circuit layer is connected to the sensor inside the battery cell, and the outer layer of the PVDF film is exposed to the external environment.

[0147] Among them, the multi-layer high-density interconnected circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external detection equipment through vertical conductive holes.

[0148] The PVDF membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring equipment through multiple layers of high-density interconnected circuit layers, thus achieving real-time monitoring of the battery's external environment.

[0149] The performance of a lithium battery prepared using the packaging film prepared in this embodiment was tested.

[0150] The packaged batteries are placed in a high temperature and high humidity environment for testing to verify the sealing performance, signal transmission performance and environmental isolation capabilities of the packaging film.

[0151] 1. Sealing performance test Testing conditions: High temperature environment: 85℃, for 72 hours.

[0152] High humidity environment: 85% relative humidity (RH) for 72 hours.

[0153] Cycle environment: high and low temperature cycle test, temperature range: -20℃~85℃, each cycle is 24 hours, a total of 10 cycles, the test results are as follows Figure 6 shown.

[0154] The helium leak detection data is: Initial helium leakage rate: 1×10 -7 cc / s ; After high temperature environment: 1.1×10 -7 cc / s ; After high humidity environment: 1.0×10 -7 cc / s ; After cycle environment: 1.2×10 -7 cc / s .

[0155] 2. Signal transmission performance test, test results such as Figure 7 shown.

[0156] Testing conditions: Normal working environment: 25℃, for 24 hours.

[0157] High temperature environment: 85℃, for 24 hours.

[0158] Low temperature environment: -20℃, for 24 hours.

[0159] Resistance test data: 25℃: 0.08Ω 85℃: 0.1Ω -20℃:0.13Ω.

[0160] 3. Environmental isolation capability test Testing conditions: High humidity environment: 85% relative humidity (RH) for 72 hours.

[0161] Salt spray environment: Salt spray test, 5% sodium chloride solution, for 48 hours.

[0162] Weight change test data: Before high humidity environment: 200.1mg After high humidity environment: 202.2mg Before salt spray environment: 200.1mg After salt spray environment: 202.7mg.

[0163] Example 4

[0164] This embodiment provides a method for preparing a battery sealing film structure. The difference from the first embodiment is that the aperture of the vertical via in this embodiment is 40 μm. The other steps are the same as the first embodiment. The specific steps are as follows: S1. Material preparation S1-1, base material: polyimide (PI) film, thickness: 25 μm.

[0165] S1-2, conductive material: copper (Cu) film, thickness: 10μm.

[0166] S1-3, Insulation material: polyimide (PI) coating, thickness: 5μm.

[0167] S1-4, Sensing membrane material: polyvinylidene fluoride (PVDF) film, thickness: 50μm.

[0168] S1-5, Packaging glue: ethylene-vinyl acetate copolymer (EVA) glue.

[0169] S2. Fabrication of high-density interconnection circuit layer S2-1. Substrate preparation: Cut the polyimide (PI) film into a suitable size and bake it at 90°C for 30 minutes to remove moisture.

[0170] S2-2. Photoresist coating: evenly coat a 2 μm thick layer of photoresist (AZ5214) on the PI film at a rotation speed of 3000 rpm for 30 seconds.

[0171] S2-3, baking: bake the photoresist at 90°C for 10 minutes.

[0172] S2-4, Exposure: Use UV exposure equipment, expose through the mask plate 100mJ / cm 2 .

[0173] S2-5, Development: Develop the exposed photoresist in developer (AZ726) for 60 seconds, rinse and dry.

[0174] S2-6, depositing copper layer: electroplating was performed on the developed PI film, the electroplating solution was copper sulfate solution, and the current density was 10 mA / cm 2 , time 10 minutes, forming a 10μm thick copper layer.

[0175] S2-7. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 2000 rpm for 30 seconds.

[0176] S2-8, hole opening: Use laser drilling equipment to open vertical via holes (Via) on the dielectric layer with a hole diameter of 40μm.

[0177] S2-9, deposit the second layer of copper: repeat the photolithography and electroplating processes to form a second layer of 10μm thick copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0178] S2-10, repeat the above steps until the desired multi-layer structure is achieved.

[0179] S2-11. Cover the surface of the multi-layer high-density interconnection circuit layer with a 5μm thick polyimide (PI) protective film at a speed of 2000rpm for 30s to ensure uniform coverage.

[0180] S3. Preparation of PVDF pressure sensing membrane S3-1. Solution preparation: Dissolve PVDF powder in dimethylacetamide (DMAc) solvent to prepare a 10 wt% solution.

[0181] S3-2, solution casting: the PVDF solution was evenly coated on the glass substrate at a rotation speed of 1000 rpm for 60 seconds.

[0182] S3-3. Drying: Bake at 60°C for 1 hour to form a uniform 50 μm thick PVDF film.

[0183] S3-4. Polarization treatment: The PVDF film is placed in an electric field for polarization treatment with an electric field strength of 1 kV / mm for 30 minutes to enhance its piezoelectric properties.

[0184] S4. Assemble the packaging film S4-1. Stack the prepared multi-layer high-density interconnection circuit layer and the PVDF pressure sensing film layer, ensuring that the multi-layer high-density interconnection circuit layer is on the upper side and the PVDF pressure sensing film layer is on the lower side.

[0185] S4-2, use EVA glue to bond the two layers to ensure a close fit; heat seal at 150°C for 5 seconds and a pressure of 0.5 MPa to ensure that the edges of the packaging film are tightly sealed to prevent air and moisture from entering, and obtain the packaging film. The prepared packaging film is applied to the packaging of lithium batteries, and the packaging film is adhered to the surface of the battery to ensure that the multi-layer high-density interconnected circuit layer is connected to the sensor inside the battery cell, and the outer layer of the PVDF film is exposed to the external environment.

[0186] Among them, the multi-layer high-density interconnected circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external detection equipment through vertical conductive holes.

[0187] The PVDF membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring equipment through multiple layers of high-density interconnected circuit layers, thus achieving real-time monitoring of the battery's external environment.

[0188] The performance of a lithium battery prepared using the packaging film prepared in this embodiment was tested.

[0189] The packaged batteries are placed in a high temperature and high humidity environment for testing to verify the sealing performance, signal transmission performance and environmental isolation capabilities of the packaging film.

[0190] 1. Sealing performance test Testing conditions: High temperature environment: 85℃, for 72 hours.

[0191] High humidity environment: 85% relative humidity (RH) for 72 hours.

[0192] Cycle environment: high and low temperature cycle test, temperature range: -20℃~85℃, each cycle is 24 hours, a total of 10 cycles, the test results are as follows Figure 8 shown.

[0193] The helium leak detection data is: Initial helium leakage rate: 1×10 -7 cc / s ; After high temperature environment: 1.3×10 -7 cc / s ; After high humidity environment: 1.1×10 -7 cc / s ; After cycle environment: 1.4×10 -7 cc / s .

[0194] 2. Signal transmission performance test, test results such as Fig. 9 shown.

[0195] Testing conditions: Normal working environment: 25℃, for 24 hours.

[0196] High temperature environment: 85℃, for 24 hours.

[0197] Low temperature environment: -20℃, for 24 hours.

[0198] Resistance test data: 25℃: 0.11Ω 85℃: 0.13Ω -20℃:0.16Ω.

[0199] 3. Environmental isolation capability test Testing conditions: High humidity environment: 85% relative humidity (RH) for 72 hours.

[0200] Salt spray environment: Salt spray test, 5% sodium chloride solution, for 48 hours.

[0201] Weight change test data: Before high humidity environment: 200.2mg After high humidity environment: 202.3mg Before salt spray environment: 200.2mg After salt spray environment: 202.9 mg.

[0202] Example 5

[0203] This embodiment provides a method for preparing a battery sealing film structure. The difference from the first embodiment is that the aperture of the vertical via in this embodiment is 60 μm. The other steps are the same as the first embodiment. The specific steps are as follows: S1. Material preparation S1-1, base material: polyimide (PI) film, thickness: 25 μm.

[0204] S1-2, conductive material: copper (Cu) film, thickness: 10μm.

[0205] S1-3, Insulation material: polyimide (PI) coating, thickness: 5μm.

[0206] S1-4, Sensing membrane material: polyvinylidene fluoride (PVDF) film, thickness: 50μm.

[0207] S1-5, Packaging glue: ethylene-vinyl acetate copolymer (EVA) glue.

[0208] S2. Fabrication of high-density interconnection circuit layer S2-1. Substrate preparation: Cut the polyimide (PI) film into a suitable size and bake it at 90°C for 30 minutes to remove moisture.

[0209] S2-2. Photoresist coating: evenly coat a 2 μm thick layer of photoresist (AZ5214) on the PI film at a rotation speed of 3000 rpm for 30 seconds.

[0210] S2-3, baking: bake the photoresist at 90°C for 10 minutes.

[0211] S2-4, Exposure: Use UV exposure equipment, expose through the mask plate 100mJ / cm 2 .

[0212] S2-5, Development: Develop the exposed photoresist in developer (AZ726) for 60 seconds, rinse and dry.

[0213] S2-6, depositing copper layer: electroplating was performed on the developed PI film, the electroplating solution was copper sulfate solution, and the current density was 10 mA / cm 2 , time 10 minutes, forming a 10μm thick copper layer.

[0214] S2-7. Dielectric layer coating: Coat a 5 μm thick polyimide (PI) coating on the copper layer at a rotation speed of 2000 rpm for 30 seconds.

[0215] S2-8, Drilling: Use laser drilling equipment to drill vertical vias (Via) on the dielectric layer with a hole diameter of 60μm.

[0216] S2-9, deposit the second layer of copper: repeat the photolithography and electroplating processes to form a second layer of 10μm thick copper conductive lines, and connect them to the first layer of lines through vertical vias.

[0217] S2-10, repeat the above steps until the desired multi-layer structure is achieved.

[0218] S2-11. Cover the surface of the multi-layer high-density interconnection circuit layer with a 5μm thick polyimide (PI) protective film at a speed of 2000rpm for 30s to ensure uniform coverage.

[0219] S3. Preparation of PVDF pressure sensing membrane S3-1. Solution preparation: Dissolve PVDF powder in dimethylacetamide (DMAc) solvent to prepare a 10 wt% solution.

[0220] S3-2, solution casting: the PVDF solution was evenly coated on the glass substrate at a rotation speed of 1000 rpm for 60 seconds.

[0221] S3-3. Drying: Bake at 60°C for 1 hour to form a uniform 50 μm thick PVDF film.

[0222] S3-4. Polarization treatment: The PVDF film is placed in an electric field for polarization treatment with an electric field strength of 1 kV / mm for 30 minutes to enhance its piezoelectric properties.

[0223] S4. Assemble the packaging film S4-1. Stack the prepared multi-layer high-density interconnection circuit layer and the PVDF pressure sensing film layer, ensuring that the multi-layer high-density interconnection circuit layer is on the upper side and the PVDF pressure sensing film layer is on the lower side.

[0224] S4-2, use EVA glue to bond the two layers to ensure a close fit; heat seal at 150°C for 5 seconds and a pressure of 0.5 MPa to ensure that the edges of the packaging film are tightly sealed to prevent air and moisture from entering, and obtain the packaging film. The prepared packaging film is applied to the packaging of lithium batteries, and the packaging film is adhered to the surface of the battery to ensure that the multi-layer high-density interconnected circuit layer is connected to the sensor inside the battery cell, and the outer layer of the PVDF film is exposed to the external environment.

[0225] Among them, the multi-layer high-density interconnected circuit layer in the packaging film is responsible for transmitting sensor signals such as temperature and pressure inside the battery cell. These signals are transmitted to external detection equipment through vertical conductive holes.

[0226] The PVDF membrane layer monitors external pressure changes in real time and transmits the pressure signal to the monitoring equipment through multiple layers of high-density interconnected circuit layers, thus achieving real-time monitoring of the battery's external environment.

[0227] The performance of a lithium battery prepared using the packaging film prepared in this embodiment was tested.

[0228] The packaged batteries are placed in a high temperature and high humidity environment for testing to verify the sealing performance, signal transmission performance and environmental isolation capabilities of the packaging film.

[0229] 1. Sealing performance test Testing conditions: High temperature environment: 85℃, for 72 hours.

[0230] High humidity environment: 85% relative humidity (RH) for 72 hours.

[0231] Cycle environment: high and low temperature cycle test, temperature range: -20℃~85℃, each cycle is 24 hours, a total of 10 cycles, the test results are as follows Fig.10 shown.

[0232] The helium leak detection data is: Initial helium leakage rate: 1×10 -7 cc / s ; After high temperature environment: 1.4×10 -7 cc / s ; After high humidity environment: 1.3×10 -7 cc / s ; After circulating environment: 1.5×10 -7 cc / s .

[0233] 2. Signal transmission performance test, test results such as Fig.11 shown.

[0234] Testing conditions: Normal working environment: 25℃, for 24 hours.

[0235] High temperature environment: 85℃, for 24 hours.

[0236] Low temperature environment: -20℃, for 24 hours.

[0237] Resistance test data: 25℃: 0.09Ω 85℃: 0.11Ω -20℃:0.14Ω.

[0238] 3. Environmental isolation capability test Testing conditions: High humidity environment: 85% relative humidity (RH) for 72 hours.

[0239] Salt spray environment: Salt spray test, 5% sodium chloride solution, for 48 hours.

[0240] Weight change test data: Before high humidity environment: 200.3mg After high humidity environment: 202.5mg Before salt spray environment: 200.3mg After salt spray environment: 203.0mg.

[0241] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A battery packaging film structure, characterized in that: It includes a high-density interconnection circuit layer and a sensor film layer, wherein the high-density interconnection circuit layer is located above the sensor film layer; the high-density interconnection circuit layer has multiple layers, each layer is separated by an insulating medium, and electrical connection between the upper and lower layers is achieved through vertical conductive holes.

2. A battery packaging film structure according to claim 1, characterized in that: The surface of the high-density interconnection circuit layer is covered with a polyimide protective film.

3. A method for preparing a battery packaging film structure, characterized in that: The following steps are involved: Prepare the substrate: Select polyimide film as the substrate; Photolithography and electroplating: The circuit pattern is defined by photolithography, and then the copper layer is deposited to form the conductive line; Stacking and vertical vias: Coating a polyimide dielectric layer on each layer of circuits, then opening vertical vias, and then depositing copper to form upper and lower layer connections; repeating this process until the desired multi-layer structure is achieved; Packaging and protection: Cover the surface of the multi-layer high-density interconnected circuit layer structure with a polyimide protective film; Solution preparation: prepare the raw materials required for preparation into a solution; Solution casting: The prepared solution is evenly coated on a glass substrate and then dried to form a sensing film; Polarization treatment: Place the sensing film in an electric field for polarization treatment; Assembly: stacking the prepared multi-layer high-density interconnection circuit layer and the sensor film, ensuring that the multi-layer high-density interconnection circuit layer is on the top and the sensor film is on the bottom, and using an adhesive to bond the multi-layer high-density interconnection circuit layer and the sensor film to ensure a close fit; Packaging: Packaging the assembled battery film to ensure that the edges of the packaging film are tightly sealed.

4. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The copper layer is deposited using an electroplating process.

5. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The packaging is done by heat sealing.

6. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The polyimide substrate for preparing multi-layer high-density interconnection circuit layers is baked at a temperature of 80°C to 100°C to remove moisture before photolithography.

7. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The thickness of the copper layer is 8μm ~12μm.

8. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The diameter of the vertical via hole is 40µm ~60µm.

9. The method for preparing a battery packaging film structure according to claim 3, characterized in that: The solution for preparing the sensing membrane is a solution of 8 wt% to 12 wt% formed by dissolving polyvinylidene fluoride in dimethylacetamide solvent.

10. A lithium battery, characterized in that: A battery packaging film structure comprising the battery packaging film structure described in any one of claims 1 to 2 or a battery packaging film structure prepared by the preparation method described in any one of claims 3 to 9.

Citation Information

Patent Citations

  • Multi-connected single lithium battery pack packaging technology

    CN109860442A

  • Flexible sensing array for monitoring multiple physical fields in lithium battery

    CN114295160A

  • Flexible sensor, lithium battery with self-heating and pressure sensing functions and manufacturing process of lithium battery

    CN115326248A

  • Flexible sensor for monitoring battery cell, monitoring device and battery unit

    CN117029913A

  • Multilayer flexible electronic integrated thin film stress metamaterial sensor and preparation method thereof