Solar-driven cathode metal protection device with modular design structure

By introducing electron transport layer, hole transport layer and hole consumption layer into photoelectrochemical cathodic protection technology, and using ZnO, ZnIn2S4 and NiFe LDH materials, the problem that a single photoelectric conversion material is difficult to meet multiple needs is solved, and efficient Cathodic protection provides stable and sustainable metal corrosion protection.

CN118765117APending Publication Date: 2024-10-11SUN YAT SEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410822300.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing photoelectrochemical cathodic protection technology, it is difficult for a single photoelectric conversion material to meet the requirements of light absorption, carrier generation, electron and hole separation, charge diffusion and hole surface oxidation reaction at the same time, which limits the efficiency of cathodic protection.

Method used

A solar-driven cathode metal protection device with a modular design structure is used. By introducing an electron transport layer, a hole transport layer and a hole consumption layer, ZnO, ZnIn2S4 and NiFe LDH materials are used to achieve directional carrier migration and rapid hole consumption. , improve photoelectric conversion efficiency and cathodic protection effect.

Benefits of technology

It achieves directional migration and efficient separation of carriers, improves cathodic protection performance, provides a green, environmentally friendly, economical and sustainable metal anti-corrosion strategy, and can stably protect 304 stainless steel for at least 2 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765117A_ABST
    Figure CN118765117A_ABST
Patent Text Reader

Abstract

The invention discloses a solar-driven cathode metal protection device with a modular design structure. The device structurally comprises a conductive substrate layer, an electron transport layer, a photoelectric conversion layer, a hole transport layer and a hole consumption layer which are sequentially arranged from bottom to top, the material used by the electron transport layer comprises ZnO, the material used by the photoelectric conversion layer comprises ZnIn2S4, the material used by the hole transport layer comprises CNTs, and the material used by the hole consumption layer comprises NiFe LDH. The solar driven cathode metal protection device is assembled layer by layer through a method from bottom to top, has the characteristics of carrier directional migration and efficient separation and rapid consumption of holes on the surface, and provides a green, environment-friendly, economic and sustainable strategy for corrosion prevention work of metal materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the intersection of cathode protection and photovoltaic application, and in particular to a solar-driven cathode metal protection device with a modular design structure. Background Art

[0002] Metal corrosion has caused serious economic losses and safety hazards to human society. Since metals are prone to lose electrons during the corrosion process, the electrochemical protection technology of metals usually uses them as cathodes and continuously supplies electrons to them to resist corrosion. Among them, impressed current cathodic protection (ICCP) and sacrificial anode cathodic protection (SACP) are widely used, but their inherent shortcomings limit their further development, such as ICCP's dependence on the power grid and huge electricity costs, SACP's continuous consumption of anode materials and the release of toxic substances into seawater. Photoelectrochemical cathodic protection (PCP) is a promising metal corrosion protection technology that can make full use of green, clean, and renewable solar energy to provide metals with a stable current to avoid corrosion through the conversion of light-electro-chemical energy. In the past two decades, PCP technology has made great progress in the field of metal protection with its low-cost, low-carbon, stable and sustainable advantages.

[0003] PCP technology is mainly divided into two types: coating method and photoanode method. The coating method refers to directly coating the photoelectric conversion material on the metal substrate, and the photoanode method refers to making the photoelectric conversion material into an electrode form and connecting it to the protected metal through an external wire. Since the coating method has high requirements for the large-scale preparation and long-term stability of photoelectric conversion materials, the process flow is cumbersome and the engineering implementation is difficult, the photoanode method is more widely used. The implementation process of PCP technology uses photoelectric conversion materials as core components. After absorbing photon energy greater than its band gap, the valence band electrons jump to the conduction band and leave holes, and the photogenerated electrons are transferred to the metal to drive the cathode protection effect. However, the stability of photoelectric conversion materials under long-term operation, sustainability in insufficient light, recombination of photogenerated carriers, and slow surface oxidation reaction of holes have largely limited their overall efficiency.

[0004] Therefore, the major challenge facing the current PCP technology is that a single photoelectric conversion material is difficult to simultaneously meet the requirements of multiple links such as light absorption and carrier generation, electron and hole separation, charge diffusion, and electron injection into the protected metal and hole injection into the surface oxidation reaction. Designing a multi-module and multifunctional integrated PCP device that efficiently captures sunlight and excites carriers, guides directional charge migration, and accelerates the oxygen evolution reaction process is an effective way to improve the overall performance of cathodic protection. Summary of the invention

[0005] In order to overcome the problems existing in the prior art, the present invention provides a new solar-driven cathode metal protection device with a modular design structure, which promotes the photoelectric conversion efficiency by introducing an electron transport layer, a hole transport layer and a hole consumption layer, thereby improving the overall protection effect of the PCP device on the target metal.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides a solar-driven cathode metal protection device with a modular design structure, wherein the structure of the device comprises a conductive substrate layer, an electron transport layer, a photoelectric conversion layer, a hole transport layer and a hole consumption layer arranged in sequence from bottom to top;

[0008] The material used for the electron transport layer includes ZnO, and the material used for the photoelectric conversion layer includes ZnIn 2 S 4 The material used for the hole transport layer includes CNTs, and the material used for the hole consumption layer includes NiFe LDH.

[0009] The device of the present invention utilizes a photoelectric conversion material (ZnIn 2 S 4 ) captures energy greater than its band gap from sunlight to form photogenerated carriers (electrons / holes); the energy bands of the electron transport material (ZnO) and the photoelectric conversion material are interlaced to form a built-in electric field, which further separates the electron-hole pairs; the dissociated photogenerated electrons and holes are collected by the electron transport material and the hole transport material (CNTs), respectively, and further transferred to the target protected metal and the location where the surface (oxidation) reaction occurs; the hole consumption material (NiFe LDH) provides surface oxidation reaction active sites for improving the surface reaction activity and accelerating the process of holes entering the oxygen evolution reaction. The present invention assembles the solar-driven cathode metal protection device layer by layer through a bottom-up method, which has the characteristics of directional carrier migration and efficient separation, and holes can be quickly consumed on the surface, providing a green, environmentally friendly, economical and sustainable strategy for the anti-corrosion of metal materials.

[0010] The present invention does not limit the specific source of NiFe LDH, which can be commercially available or prepared by existing technology.

[0011] In a specific embodiment of the present invention, nickel nitrate, iron nitrate and urea are prepared into a mixed aqueous solution, and then subjected to a hydrothermal reaction at 100-140° C. for 10-14 hours to prepare NiFe LDH.

[0012] Preferably, the ZnO, ZnIn 2 S 4 、ZnIn 2 S 4The loading amount of NiFe LDH is 0.1~0.3mg / cm 2 , 0.1~0.5mg / cm 2 , 0.1~0.3mg / cm 2 , 0.001~0.006mg / cm 2 .

[0013] Preferably, the conductive base layer includes one of FTO, ITO and AZO.

[0014] The second aspect of the present invention provides a method for preparing the solar-driven cathode metal protection device with a modular design structure, comprising the following steps:

[0015] The electron transport layer, the photoelectric conversion layer, the hole transport layer and the hole consumption layer are sequentially prepared on the conductive substrate layer by spin coating or coating.

[0016] In some specific embodiments of the present invention, the conductive substrate is ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 15 to 30 minutes in sequence, and dried at 40 to 60° C., and further plasma cleaned for 15 to 30 minutes to make the surface oxygen-philic, and then the electron transport layer, the photoelectric conversion layer, the hole transport layer, and the hole consumption layer are prepared.

[0017] Preferably, the electron transport layer material is ZnO, and an ethanol dispersion of ZnO is spin-coated on the surface of the conductive substrate layer, and the electron transport layer is obtained after vacuum drying; further preferably, the concentration of the ethanol dispersion of ZnO is 14-16 mg / mL, the spin coating speed is 2500-3500 rpm, and the spin coating time is 15-60 s.

[0018] More preferably, the vacuum drying temperature is 25-75°C.

[0019] Preferably, the photoelectric conversion layer material is ZnIn 2 S 4 , take ZnIn 2 S 4 The aqueous dispersion is coated on the surface of the electron transport layer and vacuum dried to obtain a photoelectric conversion layer.

[0020] Further preferably, the ZnIn 2 S 4 The concentration of the aqueous dispersion is 1.8 to 2.6 mg / mL; further preferably, the ZnIn 2 S 4 The concentration of the aqueous dispersion is 2.0 to 2.4 mg / mL.

[0021] Preferably, the hole transport layer material is CNTs, and a CNTs aqueous dispersion is spin-coated on the surface of the photoelectric conversion layer, and then vacuum dried to obtain the hole transport layer.

[0022] More preferably, the concentration of the CNTs aqueous dispersion is 1.5-2.0 wt. %; still more preferably, the concentration of the CNTs aqueous dispersion is 1.7-1.8 wt. %.

[0023] Preferably, the hole consumption layer material is NiFe LDH, and a NiFe LDH ethanol dispersion is coated on the surface of the hole transport layer, and then vacuum dried to obtain the hole consumption layer.

[0024] More preferably, the concentration of the NiFe LDH ethanol dispersion is 0.2-0.4 mg / mL.

[0025] In the present invention, the photoelectrochemical performance test of the device is to use the above-mentioned solar-driven cathode metal protection device with a modular design structure as the working electrode, the calomel electrode as the reference electrode, and the platinum sheet electrode as the counter electrode to form a photoelectrochemical three-electrode test system, and the electrolyte used in the test is 3.5% NaCl solution (pH 7).

[0026] In the present invention, the cathode protection performance test of the device is to use the above-mentioned solar-driven cathode metal protection device with a modular design structure as a photoanode, 304 stainless steel as a working electrode, a calomel electrode as a reference electrode, and a platinum sheet electrode as a counter electrode to form a photoelectrochemical cathode protection three-electrode test system, and the electrolyte used in the test is 3.5% NaCl solution (pH 7).

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention introduces electron / hole transport materials on the basis of traditional photoelectric conversion materials, establishes a carrier directional migration mechanism, promotes the electron-hole separation process, improves the photoelectric conversion efficiency, and achieves more efficient cathode protection.

[0029] (2) The present invention designs a hole consumption layer as a surface (oxidation) reaction catalyst to promptly eliminate the photogenerated holes accumulated on the surface interface and avoid charge recombination, which helps to improve the overall efficiency of the PCP device.

[0030] (3) The solar-driven cathode metal protection device with a modular design structure designed by the present invention can provide stable and sustainable protection for 304 stainless steel. After the device runs continuously for 2 hours or the light is switched on and off for 35 cycles (each cycle is 200 seconds), it can still provide an effective protective potential for the metal to prevent it from corrosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The manufacturing process of the solar-driven cathode metal protector with a modular design structure according to an embodiment of the present invention;

[0032] Figure 2 A schematic diagram of a solar-driven cathode metal protection device with a modular design structure;

[0033] Figure 3 This is a scanning electron microscope characterization of the cross section of Example 1;

[0034] Figure 4 ZnIn 2 S 4 UV-Vis diffuse reflectance spectrum;

[0035] Figure 5 The linear sweep voltammetry test results of Example 1, Comparative Example 1 and Comparative Example 3 in 3.5% NaCl (pH=7.0) electrolyte under intermittent illumination;

[0036] Figure 6 The open circuit potential test results of Example 1 and Comparative Examples 2 to 6 in 3.5% NaCl (pH=7.0) electrolyte under continuous illumination;

[0037] Figure 7 Polarization curve test results of Example 1 and Comparative Example 6 in 3.5% NaCl (pH=7.0) electrolyte;

[0038] Figure 8 The open circuit potential test results of Example 1 and Comparative Example 3 under continuous illumination after coupling with 304 stainless steel in 3.5% NaCl (pH=7.0) electrolyte. DETAILED DESCRIPTION

[0039] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0040] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0041] Example 1

[0042] Preparation of FTO / ETL / PCL / HTL / HCL, the steps are as follows Figure 1 As shown, the specific steps include:

[0043] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0044] Step 2: Take 15 mg ZnO, add 1 mL anhydrous ethanol, and stir ultrasonically for 60 min to make it evenly dispersed; further take 15 μL of the dispersion and spin-coat it on the aforementioned FTO surface at a spin-coating speed of 3000 rpm for 30 s; further transfer the electrode to a 50-100 ° C vacuum drying oven and dry it for 0.5-2 h to obtain FTO / ETL;

[0045] Step 3: Take 180 μL of 2.2 mg mL -1 ZnIn 2 S 4 The aqueous dispersion was evenly coated on the surface of the aforementioned FTO / ETL, and further transferred to a vacuum drying oven at 25-75°C and dried for 12 h to obtain FTO / ETL / PCL;

[0046] Step 4: Take 15 μL of 1.75 wt.% CNTs aqueous dispersion and spin-coat it on the surface of the aforementioned FTO / ETL / PCL at a spin-coating speed of 3000 rpm for 30 seconds; further transfer the electrode to a vacuum drying oven at 25-75°C and dry it for 0.5-2 hours to obtain FTO / ETL / PCL / HTL;

[0047] Step 5: Take 0.3g Ni(NO 3 ) 2 6H 2 O, 0.4 g Fe(NO 3 ) 3 9H 2 O and 0.3g urea were dissolved in 80mL deionized water, further subjected to hydrothermal reaction at 120°C for 12h, and cooled and dried to obtain NiFe LDH; 0.3mg NiFe LDH was added with 1mL anhydrous ethanol, and ultrasonic stirring was performed for 60min to make the dispersion uniform; 15μL of the dispersion was evenly coated on the surface of the aforementioned FTO / ETL / PCL / HTL, and further transferred to a vacuum drying oven at 25-75°C and dried for 0.5h to obtain FTO / ETL / PCL / HTL / HCL.

[0048] Comparative Example 1

[0049] Treatment of FTO

[0050] The size of FTO is 1.5×2.0 cm. Acetone, anhydrous ethanol, and deionized water are used to ultrasonically clean FTO for 15 to 30 minutes, and then plasma cleaning is performed for 30 minutes to obtain a clean substrate electrode FTO.

[0051] Comparative Example 2

[0052] The preparation of FTO / ETL includes the following steps:

[0053] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0054] Step 2: Take 15 mg ZnO, add 1 mL anhydrous ethanol, and stir ultrasonically for 60 min to make it evenly dispersed; further take 15 μL of the dispersion and spin coat it on the aforementioned FTO surface at a spin coating speed of 3000 rpm for 30 s; further transfer the electrode to a 50-100 ° C vacuum drying oven and dry it for 0.5-2 h to obtain FTO / ETL.

[0055] Comparative Example 3

[0056] The preparation of FTO / PCL includes the following steps:

[0057] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0058] Step 2: Take 180 μL of 2.2 mg mL -1 ZnIn 2 S 4 The aqueous dispersion was evenly coated on the surface of the aforementioned FTO, and further transferred to a vacuum drying oven at 25-75° C. and dried for 12 h to obtain FTO / PCL.

[0059] Comparative Example 4

[0060] The preparation of FTO / HTL includes the following steps:

[0061] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0062] Step 2: Take 15 μL of 1.75 wt.% CNTs aqueous dispersion and spin coat it on the FTO surface at a speed of 3000 rpm for 30 s. Then transfer the electrode to a vacuum drying oven at 25-75°C and dry for 0.5-2 h to obtain FTO / HTL.

[0063] Comparative Example 5

[0064] The preparation of FTO / ETL / PCL includes the following steps:

[0065] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0066] Step 2: Take 15 mg ZnO, add 1 mL anhydrous ethanol, and stir ultrasonically for 60 min to make it evenly dispersed; further take 15 μL of the dispersion and spin-coat it on the aforementioned FTO surface at a spin-coating speed of 3000 rpm for 30 s; further transfer the electrode to a 50-100 ° C vacuum drying oven and dry it for 0.5-2 h to obtain FTO / ETL;

[0067] Step 3: Take 180 μL of 2.2 mg mL -1 ZnIn 2 S 4 The aqueous dispersion was evenly coated on the surface of the aforementioned FTO / ETL, and further transferred to a vacuum drying oven at 25-75° C. and dried for 12 hours to obtain FTO / ETL / PCL.

[0068] Comparative Example 6

[0069] The preparation of FTO / ETL / PCL / HTL includes the following steps:

[0070] Step 1: The size of FTO is 1.5×2.0 cm. Use acetone, anhydrous ethanol, and deionized water to ultrasonically clean FTO for 15 to 30 minutes, and then plasma clean it for 30 minutes;

[0071] Step 2: Take 15 mg ZnO, add 1 mL anhydrous ethanol, and stir ultrasonically for 60 min to make it evenly dispersed; further take 15 μL of the dispersion and spin-coat it on the aforementioned FTO surface at a spin-coating speed of 3000 rpm for 30 s; further transfer the electrode to a 50-100 ° C vacuum drying oven and dry it for 0.5-2 h to obtain FTO / ETL;

[0072] Step 3: Take 180 μL of 2.2 mg mL -1 ZnIn 2 S 4 The aqueous dispersion was evenly coated on the surface of the aforementioned FTO / ETL, and further transferred to a vacuum drying oven at 25-75°C and dried for 12 h to obtain FTO / ETL / PCL;

[0073] Step 4: Take 15 μL of 1.75wt.% CNTs aqueous dispersion and spin coat it on the surface of the aforementioned FTO / ETL / PCL at a spin coating speed of 3000 rpm for 30 seconds; further transfer the electrode to a vacuum drying oven at 25-75°C and dry for 0.5-2 hours to obtain FTO / ETL / PCL / HTL.

[0074] The morphology of the modular device was characterized by scanning electron microscopy. Figure 3 As shown in the cross-sectional image of Example 1, it can be seen that the tubular interwoven structure of the top layer is CNTs, and the wrinkled sheet-like stacked structure of the middle layer is ZnIn 2 S 4 , the densely packed nanoparticles in the lower layer are ZnO. In addition, ZnIn 2 S 4 The UV-Vis diffuse reflectance spectrum is as follows Figure 4 As shown, its absorption edge is located near 563nm and has visible light absorption characteristics.

[0075] Photoelectrochemical tests were carried out on Example 1, Comparative Example 1 and Comparative Example 3, and the linear sweep voltammetric test results are as follows: Figure 5 As shown, no photoelectric response was observed in Comparative Example 1; an obvious photoelectric signal appeared in Comparative Example 3, indicating that the PCL functional module was successfully fixed; after further assembling ETL, HTL and HCL, the photoelectric response of Example 1 was significantly enhanced, indicating that the introduction of multiple functional modules is conducive to the collection of photogenerated carriers. Open circuit voltage tests were carried out on Example 1 and Comparative Examples 2 to 6, and the results are as follows Figure 6 As shown, Comparative Example 4 has no photoelectric response, which is attributed to the fact that HTL is not a semiconductor material; Comparative Examples 2, 3, 5 and 6 all observed photoinduced potential drop. As the number of assembled modules gradually increased, the degree of open circuit potential drop increased significantly, indicating that the prepared FTO / ETL / PCL / HTL / HCL has excellent photoelectrochemical performance as a cathode protection device. The catalytic performance of Example 1 and Comparative Example 6 was further investigated, and the polarization curve test results are shown in Figure 7 At the same potential, due to the presence of HCL, the current density obtained in Example 1 is significantly greater than that in Comparative Example 6. The corresponding Tafel slopes are calculated to be 30.8 mV·dec. -1 (Example 1) and 33.5mV·dec -1 (Comparative Example 6) shows that NiFeLDH has a certain promoting effect on the surface oxidation reaction of holes, and the prepared FTO / ETL / PCL / HTL / HCL has good catalytic kinetics as a cathode protection device.

[0076] The cathodic protection performance of the prepared device was investigated, and the open circuit potential curves of Example 1 and Comparative Example 3 were tested after long-term operation after coupling with 304 stainless steel. Figure 8 As shown, under continuous lighting conditions, Comparative Example 3 can significantly reduce the potential of 304 stainless steel in the initial stage, but as the working time increases, the potential of 304 stainless steel quickly shifts positively; in the initial stage, the ability of Example 1 to reduce the potential of 304 stainless steel is significantly better than that of Comparative Example 3, and as the test time increases, the speed of the positive shift of the potential of 304 stainless steel is significantly slower than that coupled with Comparative Example 3, indicating that the multi-module layer-by-layer assembly structure of the device can effectively delay the loss of photoelectric conversion materials, and the cathode protection effect of the prepared device can be maintained for at least 2 hours, showing good stability and sustainability.

[0077] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A solar-driven cathode metal protection device with a modular design structure, characterized in that: The structure of the device includes a conductive substrate layer, an electron transport layer, a photoelectric conversion layer, a hole transport layer and a hole consumption layer arranged in sequence from bottom to top; The material used for the electron transport layer includes ZnO, the material used for the photoelectric conversion layer includes ZnIn2S4, the material used for the hole transport layer includes CNTs, and the material used for the hole consumption layer includes NiFe LDH.

2. The solar-driven cathode metal protection device with a modular design structure according to claim 1, characterized in that: The loading amounts of ZnO, ZnIn2S4, ZnIn2S4 and NiFe LDH are 0.1-0.3 mg / cm 2 , 0.1~0.5mg / cm 2 , 0.1~0.3mg / cm 2 , 0.001~0.006mg / cm 2 .

3. The solar-driven cathode metal protection device with a modular design structure according to claim 1, characterized in that: The conductive substrate layer includes one of FTO, ITO and AZO.

4. A method for preparing a solar-driven cathode metal protection device with a modular design structure according to any one of claims 1 to 3, characterized in that: The following steps are involved: The electron transport layer, the photoelectric conversion layer, the hole transport layer and the hole consumption layer are sequentially prepared on the conductive substrate layer by spin coating or coating.

5. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 4, characterized in that: The electron transport layer material is ZnO, and an ethanol dispersion of ZnO is spin-coated on the surface of the conductive substrate layer, and the electron transport layer is obtained after vacuum drying.

6. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 4, characterized in that: The photoelectric conversion layer material is ZnIn2S4. A ZnIn2S4 aqueous dispersion is coated on the surface of the electron transport layer, and the photoelectric conversion layer is obtained after vacuum drying.

7. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 6, characterized in that: The concentration of the ZnIn2S4 aqueous dispersion is 1.8-2.6 mg / mL.

8. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 4, characterized in that: The hole transport layer material is CNTs, and a CNTs aqueous dispersion is spin-coated on the surface of the photoelectric conversion layer, and the hole transport layer is obtained after vacuum drying.

9. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 8, characterized in that: The concentration of the CNTs aqueous dispersion is 1.5-2.0 wt.%.

10. The method for preparing a solar-driven cathode metal protection device with a modular design structure according to claim 4, characterized in that: The hole consumption layer material is NiFe LDH, and a NiFe LDH ethanol dispersion is coated on the surface of the hole transport layer, and the hole consumption layer is obtained after vacuum drying.

Citation Information

Patent Citations

  • Preparation of double-layer energy storage type photoanode and application of double-layer energy storage type photoanode in metal cathode protection

    CN111663140A

  • Nano grass composite photoelectric material for photoelectrochemical cathode protection and preparation and application of nano grass composite photoelectric material

    CN112921324A

  • Energy storage type semiconductor composite photoanode for metal corrosion protection