Interface modified perovskite solar cell and preparation method thereof
By using organic hydrochloride molecules as interface modifiers in perovskite solar cells, the problems of high-density defects and poor energy level matching of perovskite solar cells are solved, their efficiency and stability are improved, and efficient carriers are achieved. Current transport and long-term photostability.
Patent Information
- Application Number
- CN202411122730.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-29
AI Technical Summary
Perovskite solar cells have high density of defects and poor energy level matching, which limits their photoelectric conversion efficiency and stability. In particular, defects on the surface of the perovskite film and the energy level difference between the interfaces lead to reduced device performance.
Organic hydrochloride molecules are used as interface modifiers, and an interface modification layer is formed on the surface of the perovskite light-absorbing layer through dynamic spin coating technology, which effectively passivates positive charge defects, improves interface energy level matching, and promotes carrier extraction and transmission.
Improved the efficiency and stability of perovskite solar cells, with the championship efficiency reaching 22.28% and maintaining an initial efficiency of 84.1% after 500 hours of illumination, significantly improving the energy level matching between the electron transport layer and the perovskite film. Charge transfer.
Smart Images

Figure CN118870833A_ABST
Abstract
Description
Technical field:
[0001] The present invention relates to the technical field of solar cells, and in particular to an interface-modified perovskite solar cell and a preparation method thereof. Background technology:
[0002] Organic-inorganic lead halide perovskite solar cells (PSCs) have attracted widespread attention in the field of scientific research and commercial applications due to their excellent photoelectric conversion efficiency (PCE) and relatively inexpensive preparation methods. Among them, inverted structure PSCs have attracted widespread attention from researchers because of their simpler preparation process, lower cost, low-temperature film formation, and no obvious hysteresis effect. Nevertheless, the high-density defects on the surface of perovskite films and the energy level difference between interfaces significantly limit their photoelectric conversion efficiency and operational stability. Therefore, finding cost-effective interface modifiers is crucial for the further commercial development of PSCs.
[0003] Studies have shown that due to the low formation energy of defects in perovskites, the perovskite film formation process often leads to defects on the film surface, which is attributed to the insufficient stability of organic amine cations and iodide-triiodide redox reactions. In addition, fullerene derivatives are widely used in electron transport layers, but these derivatives still have many shortcomings to be overcome, such as poor coverage of the electron transport layer material PCBM on the perovskite film, weak water barrier ability, poor energy level matching, and poor interface contact, which hinders device performance and reduces the life of the device. Therefore, interface engineering aimed at improving the stability of the perovskite / electron transport layer interface becomes crucial. Summary of the invention:
[0004] The present invention solves the problems of high-density defects and poor energy level matching in perovskite solar cells, and provides an interface-modified perovskite solar cell and a preparation method thereof. The interface modification layer can improve the efficiency of the perovskite solar cell (the champion efficiency reaches 22.28%), and at the same time improve the stability of the perovskite solar cell (under a standard sunlight in a nitrogen environment, the initial efficiency is still maintained at 84.1% after 500 hours of continuous illumination maximum power point tracking test (MPPT)).
[0005] The first object of the present invention is to provide an interface-modified perovskite solar cell, wherein the perovskite solar cell is a pin-type structure, comprising a transparent conductive substrate, a hole transport layer, a perovskite light-absorbing layer, an interface modification layer, an electron transport layer, a hole blocking layer and an electrode layer stacked in sequence from bottom to top; the material of the interface modification layer is an organic hydrochloride molecule solution, and the organic hydrochloride molecule is an organic hydrochloride molecule having an amino group and a benzene ring, wherein the amino group is directly connected to the benzene ring and the para-position of the amine group is an electron-withdrawing group.
[0006] The interface modification material proposed in the present invention can effectively passivate positive charge defects (uncoordinated Pb 2+ and iodine ion vacancies), improving the interface energy level matching and promoting carrier extraction and transport.
[0007] Preferably, the organic hydrochloride molecule is selected from one or two of 4-aminobenzoic acid ethyl ester hydrochloride (benzocaine hydrochloride), 2-diethylaminoethyl 4-aminobenzoate hydrochloride (procaine hydrochloride), 4-aminobenzoic acid hydrochloride and 4-aminobenzoic acid methyl ester hydrochloride.
[0008] Preferably, the interface modification layer is prepared by the following steps: dynamically spin-coating an organic hydrochloride molecular solution onto the surface of the perovskite light-absorbing layer to obtain the interface modification layer; the solvent of the organic hydrochloride molecular solution is isopropanol, and the concentration of the organic hydrochloride molecular solution is 0.1 to 1.5 mg / mL.
[0009] More preferably, the conditions of the dynamic spin coating are: a spin coating speed of 3000 to 7000 rpm and a spin coating time of 20 to 60 s.
[0010] Preferably, the thickness of the interface modification layer is 2-10 nm.
[0011] Preferably, the transparent conductive substrate is selected from one of ITO conductive glass, FTO conductive glass, and transparent conductive flexible plastic. Further preferably, the transparent conductive substrate is selected from FTO transparent conductive glass, ITO transparent conductive glass, ITO transparent conductive PEN, or ITO transparent conductive PET.
[0012] Preferably, the material of the hole transport layer is nickel oxide, 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-diphenyl-9H-carbazole-9-yl)ethyl]phosphonic acid and (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid, or a mixture of the above materials.
[0013] Preferably, the material of the perovskite light absorbing layer is metal halide perovskite, the crystal structure of the metal halide perovskite is ABX3, A is selected from at least one of organic cations and inorganic cations, B is selected from divalent metal ions, and X is selected from halogen ions; the material of the electron transport layer is selected from PCBM, C 60 One of them.
[0014] Preferably, the material of the hole blocking layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline; the material of the electrode layer is selected from one of aluminum, silver and copper. The hole blocking layer is formed by evaporating the electron transport layer by thermal evaporation or by solution deposition.
[0015] The present invention also protects a method for preparing the interface-modified perovskite solar cell, comprising the following steps:
[0016] S1. Preparing a hole transport layer on the surface of a transparent conductive substrate by vacuum deposition or solution deposition;
[0017] S2, preparing a perovskite light absorbing layer by coating the surface of the hole transport layer;
[0018] S3, preparing an interface modification layer on the surface of the perovskite light-absorbing layer by dynamically spin-coating an organic hydrochloride molecular solution;
[0019] S4, preparing an electron transport layer on the surface of the interface modification layer by vacuum deposition or solution deposition;
[0020] S5, preparing a hole blocking layer on the surface of the electron transport layer by vacuum deposition or solution deposition;
[0021] S6. Prepare an electrode layer on the surface of the hole blocking layer by evaporation method to obtain the perovskite solar cell.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. The interface modification layer proposed in the present invention reduces the surface work function of the perovskite and makes it more n-type, which improves the energy level matching between the electron transport layer and the perovskite film, resulting in an increase in the open circuit voltage and improved charge extraction and transport.
[0024] 2. The introduction of the interface modification layer proposed in the present invention effectively passivates the interface defect sites in the perovskite solar cell due to the strong chemical bonding between the organic hydrochloride molecules and the perovskite surface, thereby suppressing the non-radiative recombination loss.
[0025] 3. The present invention uses organic hydrochloride molecules to modify the surface of the perovskite light-absorbing layer. After treating the surface of the perovskite light-absorbing layer, the morphological change of the perovskite film is negligible, but it triggers the surface energy level optimization and defect passivation effect, which promotes the extraction of charge carriers. This improved band alignment is conducive to the efficient extraction of electrons, which is crucial to improving the overall efficiency and performance of perovskite solar cells because it reduces energy losses at the interface and inhibits recombination. In addition, the introduction of the organic hydrochloride molecule modification layer improves the band alignment while maintaining the hole-accepting properties of the perovskite surface, and does not cause the typical iodine vacancy VI The large work function drop caused by the defects will suppress the accumulation of holes at the interface between the perovskite and the electron transport layer. This effect is beneficial for the interface between the perovskite and the electron transport layer, because it was previously found that suboptimal passivators leave too many holes at this interface, which may lead to the formation of undesirable charged Frenkel defects (CFD). Due to the strong chemical bonding of the drug to the perovskite surface, the grain boundaries are effectively passivated, thereby reducing the concentration of defect sites, which is reflected in the improved photostability, thereby reducing the non-radiative recombination of carriers at the interface, which is more conducive to charge transport and improves device stability, which provides a bright prospect for obtaining high-efficiency perovskite solar cells. Description of the drawings:
[0026] Figure 1 The perovskite solar cells prepared in Example 1, Example 2 and Comparative Example 1 of the present invention are subjected to a solar simulator (standard light source) with a light intensity of 100 mW / cm 2 The JV curve below, where J is the photocurrent density and V is the photovoltage. Specific implementation method:
[0027] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0028] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0029] The invention provides a perovskite solar cell with an organic hydrochloride molecule interface modification, which is a pin-type structure and comprises a transparent conductive substrate, a hole transport layer, a perovskite light absorbing layer, an interface modification layer, an electron transport layer, a hole blocking layer and an electrode layer stacked in sequence from bottom to top.
[0030] In the present invention, the material of the transparent conductive substrate is preferably selected from ITO transparent conductive glass, FTO transparent conductive glass, ITO transparent conductive PEN or ITO transparent conductive PET; the square resistance of the transparent conductive substrate is preferably 7 to 30Ωsq -1 , preferably 7Ωsq -1 .
[0031] In the present invention, the material of the hole transport layer is preferably selected from nickel oxide, 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-diphenyl-9H-carbazole-9-yl)ethyl]phosphonic acid and (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid, or a stacked material formed by the above materials; the material of the hole transport layer is preferably selected from nickel oxide, 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid; the thickness of the hole transport layer is preferably 50 to 150 nm, more preferably 80 to 120 nm, and most preferably 100 nm.
[0032] In the present invention, the solute in the perovskite solution is preferably selected from cesium iodide, lead iodide, dimethylamine hydroiodide, etc.; the solvent in the perovskite solution is preferably selected from one or more of DMF (N,N-dimethylformamide) and DMSO (dimethyl sulfoxide); the molar concentration of the perovskite solution is preferably 1.2-1.6 mol / L, more preferably 1.3-1.5 mol / L.
[0033] In the present invention, the perovskite solution is preferably dropped onto the hole transport layer for two-step spin coating; the rotation speed during the two-step spin coating is preferably 500-1500rpm and 4000-6000rpm, and most preferably 1000rpm and 5000rpm; the time for the two-step spin coating is preferably 5-15s and 20-40s, and most preferably 10s and 30s.
[0034] In the present invention, the material of the interface modification layer is in the form of hydrochloride, having an amino group and a benzene ring, wherein the amino group is directly connected to the benzene ring and the amino group is located at the opposite position and has an electron-withdrawing group, preferably one or two selected from 4-aminobenzoic acid ethyl hydrochloride (benzocaine hydrochloride), 2-diethylaminoethyl 4-aminobenzoate hydrochloride (procaine hydrochloride), 4-aminobenzoic acid hydrochloride and 4-aminobenzoic acid methyl ester hydrochloride.
[0035] In the present invention, the thickness of the interface modification layer is preferably 2 to 10 nm, more preferably 4 to 8 nm, and most preferably 5 to 6 nm.
[0036] In the present invention, the material of the electron transport layer is preferably selected from one of PCBM and C60.
[0037] In the present invention, the thickness of the electron transport layer is preferably 100 to 300 nm, more preferably 150 to 250 nm, and most preferably 200 nm.
[0038] In the present invention, the material of the hole blocking layer is preferably selected from 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline.
[0039] In the present invention, the thickness of the hole blocking layer is preferably 2 to 10 nm, more preferably 4 to 8 nm, and most preferably 5 nm.
[0040] In the present invention, the material of the electrode layer is preferably selected from aluminum, silver, and copper. The thickness of the electrode layer is preferably 50 to 150 nm, more preferably 80 to 120 nm, and most preferably 100 nm.
[0041] The present invention provides a method for preparing an interface-modified perovskite solar cell, comprising the following steps:
[0042] S1. preparing a hole transport layer on the surface of a transparent conductive substrate;
[0043] S2, preparing a perovskite light absorbing layer by coating the hole transport layer surface;
[0044] S3, preparing an interface modification layer on the surface of the perovskite light absorbing layer by dynamically spin coating an organic hydrochloride molecular solution;
[0045] S4, preparing an electron transport layer on the surface of the interface modification layer by vacuum deposition or solution deposition;
[0046] S5, preparing a hole blocking layer on the surface of the electron transport layer by vacuum deposition or solution deposition;
[0047] S6. Prepare an electrode layer on the surface of the hole blocking layer by evaporation method.
[0048] In the present invention, the transparent conductive substrate is preferably an ITO glass substrate, and the substrate is preferably cleaned and treated; the cleaning is preferably performed once using a glass cleaner plus deionized water, deionized water, ethanol and isopropanol; after cleaning, it is preferably blown dry; the treatment is preferably ultraviolet-ozone treatment; the treatment time is preferably 10 to 20 minutes, more preferably 15 minutes.
[0049] In the present invention, the preparation method of the hole transport layer is preferably selected from chemical bath deposition, atomic layer deposition or spin coating, more preferably spin coating.
[0050] In the present invention, the method for preparing the hole transport layer preferably comprises: diluting a commercially available aqueous solution of nickel oxide nanoparticles with deionized water to 5 mg / mL-20 mg / mL, preferably 10 mg / mL.
[0051] In the present invention, the diluted aqueous solution of nickel oxide nanoparticles is filtered and then spin-coated onto a conductive substrate, and then annealed and dried to obtain a hole transport layer. The spin coating time is preferably 25 to 35 seconds, the rotation speed is preferably 1000 to 4000 rpm, the spin coating time is more preferably 30 seconds, and the rotation speed is more preferably 2000 rpm. The annealing temperature is preferably 50°C to 150°C, more preferably 100°C; the annealing time is preferably 10 to 20 minutes, more preferably 15 minutes. Dry at 100°C for 15 minutes to obtain a hole transport layer. The thickness of the hole transport layer is preferably 10 to 40 nm, more preferably 10 nm or 40 nm.
[0052] In the present invention, the method for preparing the perovskite light absorbing layer preferably comprises: coating the perovskite solution on the surface of the hole transport layer and then annealing to obtain the perovskite light absorbing layer. The thickness of the perovskite layer is preferably 500-800nm, more preferably 500nm, 650nm or 800nm.
[0053] In the present invention, the solute in the perovskite solution is preferably selected from cesium iodide, lead iodide, dimethylamine hydroiodide, etc.; the solvent in the perovskite solution is preferably selected from one or more of DMF (N,N-dimethylformamide) and DMSO (dimethyl sulfoxide); the molar concentration of the perovskite solution is preferably 1.2-1.6 mol / L, more preferably 1.3-1.5 mol / L.
[0054] In the present invention, the perovskite solution is preferably dropped onto the substrate (interface modification layer) for two-step spin coating; the rotation speed during the two-step spin coating is preferably 500-1500rpm and 4000-6000rpm, and most preferably 1000rpm and 5000rpm; the time for the two-step spin coating is preferably 5-15s and 20-40s, and most preferably 10s and 30s.
[0055] In the present invention, the annealing temperature of the perovskite is preferably 100° C.; the annealing time is preferably 30 to 90 min, and most preferably 60 min.
[0056] In the present invention, the method for preparing the interface modification layer preferably comprises: dynamically spin-coating an organic hydrochloride molecular solution onto the surface of the perovskite light-absorbing layer and then performing a heat treatment to obtain the interface modification layer.
[0057] In the present invention, the solvent in the organic hydrochloride molecule solution is preferably selected from isopropanol; the concentration of the organic hydrochloride molecule solution is preferably 0.1-1.5 mg / mL, more preferably 0.5-1.0 mg / mL, and most preferably 0.75 mg / mL. In the present invention, the method for preparing the organic hydrochloride molecule solution preferably includes: dissolving the organic hydrochloride molecules in a solvent to obtain a solution required for interface modification; the composition of the solution is consistent with that described in the above technical solution, and will not be repeated here.
[0058] In the present invention, the rotation speed of dynamic spin coating is preferably 3000-7000 rpm, more preferably 4000-6000 rpm, and most preferably 5000 rpm; the spin coating time is preferably 20-40 s, more preferably 25-35 s, and most preferably 30 s. The thickness of the interface modification layer is preferably 2-10 nm, more preferably 4-5 nm, 5-6 nm, or 6-8 nm.
[0059] In the present invention, the method for preparing the electron transport layer preferably comprises: spin coating a precursor solution on the surface of the interface modification layer to obtain the electron transport layer. The thickness of the electron transport layer is preferably 30 to 300 nm, more preferably 30 nm, 100 nm or 300 nm.
[0060] In the present invention, the solute in the precursor solution is preferably selected from PCBM; the solvent in the precursor solution is preferably selected from chlorobenzene; the mass concentration of the precursor solution is preferably 10-30 mg / mL, preferably 15-25 mg / mL, and more preferably 20 mg / mL.
[0061] In the present invention, the spin coating rotation speed is preferably 2500-3500 rpm, more preferably 2800-3200 rpm, and most preferably 3000 rpm; the spin coating time is preferably 20-40 s, more preferably 25-35 s, and most preferably 30 s.
[0062] In the present invention, the method for preparing the hole blocking layer preferably comprises: spin coating a precursor solution on the surface of the perovskite light absorbing layer to obtain the hole blocking layer. The thickness of the hole blocking layer is preferably 2 to 10 nm, more preferably 2 nm, 5 nm or 10 nm.
[0063] In the present invention, the solute in the precursor solution is preferably selected from BCP; the solvent in the precursor solution is preferably selected from isopropanol; the mass concentration of the precursor solution is preferably 0.1-1.0 mg / mL, more preferably 0.3-0.7 mg / mL, and most preferably 0.5 mg / mL.
[0064] In the present invention, the spin coating rotation speed is preferably 2500-3500 rpm, more preferably 2800-3200 rpm, and most preferably 3000 rpm; the spin coating time is preferably 20-40 s, more preferably 25-35 s, and most preferably 30 s.
[0065] In the present invention, the method for preparing the electrode layer preferably comprises: preparing the electrode layer on the hole blocking layer by vacuum evaporation.
[0066] In the present invention, the material of the electrode layer is preferably selected from one of aluminum, silver and copper, and more preferably silver.
[0067] In the present invention, the vacuum degree during vacuum evaporation is preferably less than 10 -4 Pa, the deposition rate is preferably More preferably
[0068] The thickness of the electrode layer is preferably 50 to 150 nm, more preferably 80 to 120 nm, and most preferably 100 nm.
[0069] Example 1
[0070] The ITO glass substrate was cleaned with glass cleaner plus deionized water, deionized water, ethanol and isopropanol in turn, dried with nitrogen and then treated with UV-ozone for 15 minutes. The commercially purchased nickel oxide nanoparticle aqueous solution was diluted to 10 mg / mL with deionized water, filtered and spin-coated on the conductive glass layer (ITO glass), the spin coating time was 30s, the rotation speed was 3000rpm, and dried at 100°C for 30min to obtain a hole transport layer.
[0071] The perovskite precursor solution was spin-coated onto the hole transport layer in a nitrogen glove box (two-step spin coating, the first spin coating time was 10 s, the rotation speed was 1000 rpm, and the second spin coating time was 30 s, the rotation speed was 4000 rpm). Chlorobenzene was added as an anti-solvent during the spin coating process, and then annealed at 100 ° C for 60 min to form a perovskite polycrystalline film; the perovskite composition was Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(I 0.83 Br 0.17 )3. The perovskite precursor solution was prepared by dissolving PbI2 (0.5739 g), FAI (0.1998 g), MABr (0.0267 g), PbBr2 (0.0874 g) and CsI in 1 mL of DMF:DMSO (volume ratio 3:1) solution and stirring on a stirring table for 2 h before use. The concentration of 0.75 mg mL -1 The benzocaine hydrochloride solution was dynamically spin-coated onto the surface of the electron transport layer to obtain an interface modification layer. The rotation speed of the dynamic spin coating was 5000 rpm and the spin coating time was 30 s.
[0072] PCBM (20 mg / mL) was spin-coated at 3000 rpm for 30 s on the interface modification layer to obtain an electron transport layer.
[0073] BCP (0.5 mg / mL) was spin-coated at 3000 rpm for 30 s on the electron transport layer to obtain a hole blocking layer.
[0074] Finally, the silver electrode was prepared by vacuum evaporation, and the vacuum degree was less than 10 -4Pa, deposition rate Obtained perovskite solar cell.
[0075] In perovskite solar cells, the hole transport layer is 40nm, the perovskite layer is 650nm, the thickness of the interface modification layer is 5-6nm, the electron transport layer is 30nm, the hole blocking layer is 5nm, and the silver electrode is 100nm.
[0076] Comparative Example 1:
[0077] A perovskite solar cell was prepared according to the method of Example 1, which differs from Example 1 in that there is no interface modification layer. The device has a champion efficiency of 19.98%, and maintains 59.8% of the initial efficiency after continuous illumination MPPT for 500 hours under a standard sunlight in a nitrogen environment.
[0078] Embodiment 2:
[0079] A perovskite solar cell was prepared according to the method of Example 1. The difference from Example 1 is that the organic molecule solution is 2-diethylaminoethyl 4-aminobenzoate hydrochloride (procaine hydrochloride) with a concentration of 0.75 mg / mL, and the thickness of the interface modification layer is 5 to 6 nm.
[0080] Depend on Figure 1 It was concluded that, compared with Comparative Example 1 and Example 1, the perovskite solar cell modified with procaine hydrochloride (Example 2) exhibited better device performance, with the device champion efficiency reaching 22.28%, and maintaining 84.1% of the initial efficiency after 500 hours of continuous illumination MPPT under one standard sunlight in a nitrogen environment.
[0081] Embodiment 3:
[0082] A perovskite solar cell was prepared according to the method of Example 1. The difference from Example 1 is that the organic molecule solution is 4-aminobenzoic acid hydrochloride with a concentration of 0.75 mg / mL, and the thickness of the interface modification layer is 5 to 6 nm.
[0083] Embodiment 4:
[0084] A perovskite solar cell was prepared according to the method of Example 1. The difference from Example 1 is that the organic molecule solution is 4-aminobenzoic acid methyl ester hydrochloride with a concentration of 0.75 mg / mL, and the thickness of the interface modification layer is 5 to 6 nm.
[0085] Table 1 summarizes the main performances of the devices of Examples 1-4.
[0086] Table 1
[0087]
[0088] Embodiment 5:
[0089] A perovskite solar cell was prepared according to the method of Example 1, which differs from Example 1 in that:
[0090] The preparation of the hole transport layer includes: diluting a commercially purchased nickel oxide nanoparticle aqueous solution with deionized water to 5 mg / mL, filtering and spin-coating it onto a conductive glass layer (ITO glass), the spin coating time is 30 s, the rotation speed is 3000 rpm, and drying at 100°C for 30 min to obtain a hole transport layer.
[0091] The preparation of the perovskite light-absorbing layer includes: dropping the perovskite solution on the substrate (interface modification layer) for two-step spin coating; the rotation speeds during the two-step spin coating are 500 rpm and 4000 rpm respectively; the time of the two-step spin coating is 15 s and 40 s respectively, the annealing temperature is 100° C.; and the annealing time is 30 minutes.
[0092] The preparation of the interface modification layer includes: the concentration of the organic hydrochloride molecule solution is preferably 0.5 mg / mL.
[0093] The preparation of the electron transport layer includes: spin coating PCBM (20 mg / mL) on the interface modification layer at 2500 rpm for 30 seconds to obtain the electron transport layer.
[0094] The preparation of the hole blocking layer includes: spin coating BCP (0.3 mg / mL) on the electron transport layer at 2500 rpm for 30 seconds to obtain the hole blocking layer.
[0095] The preparation of the electrode layer includes: the vacuum degree during vacuum evaporation is less than 10 -4 Pa, the deposition rate is
[0096] In perovskite solar cells, the hole transport layer is 10nm, the perovskite layer is 500nm, the thickness of the interface modification layer is 4-5nm, the electron transport layer is 100nm, the hole blocking layer is 2nm, and the silver electrode is 50nm.
[0097] Embodiment 6:
[0098] A perovskite solar cell was prepared according to the method of Example 1, which differs from Example 1 in that:
[0099] The preparation of the hole transport layer includes: diluting a commercially purchased nickel oxide nanoparticle aqueous solution with deionized water to 20 mg / mL, filtering and spin-coating it onto a conductive glass layer (ITO glass), the spin coating time is 30 s, the rotation speed is 3000 rpm, and drying at 100°C for 30 min to obtain a hole transport layer.
[0100] The preparation of the perovskite light-absorbing layer includes: dropping the perovskite solution on the substrate (interface modification layer) for two-step spin coating; the rotation speeds during the two-step spin coating are 500 rpm and 4000 rpm respectively; the time of the two-step spin coating is 15 s and 40 s respectively, the annealing temperature is 100° C.; and the annealing time is 30 minutes.
[0101] The preparation of the interface modification layer includes: the concentration of the organic hydrochloride molecule solution is preferably 1.0 mg / mL.
[0102] The preparation of the electron transport layer includes: spin coating PCBM (20 mg / mL) on the interface modification layer at 3500 rpm for 30 seconds to obtain the electron transport layer.
[0103] The preparation of the hole blocking layer includes: spin coating BCP (0.7 mg / mL) on the electron transport layer at 3500 rpm for 30 seconds to obtain the hole blocking layer.
[0104] The preparation of the electrode layer includes: the vacuum degree during vacuum evaporation is less than 10 -4 Pa, the deposition rate is
[0105] In perovskite solar cells, the hole transport layer is 40nm, the perovskite layer is 800nm, the thickness of the interface modification layer is 6-8nm, the electron transport layer is 300nm, the hole blocking layer is 10nm, and the silver electrode is 150nm.
[0106] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. An interface-modified perovskite solar cell, characterized in that: The perovskite solar cell is a pin-type structure, comprising a transparent conductive substrate, a hole transport layer, a perovskite light-absorbing layer, an interface modification layer, an electron transport layer, a hole blocking layer and an electrode layer stacked in sequence from bottom to top; the material of the interface modification layer is an organic hydrochloride molecular solution, and the organic hydrochloride molecule is an organic hydrochloride molecule having an amino group and a benzene ring, wherein the amino group is directly connected to the benzene ring and the amino group is an electron-withdrawing group at the opposite position.
2. The perovskite solar cell according to claim 1, characterized in that The organic hydrochloride molecule is selected from one or two of ethyl 4-aminobenzoate hydrochloride, 2-diethylaminoethyl 4-aminobenzoate hydrochloride, 4-aminobenzoate hydrochloride and methyl 4-aminobenzoate hydrochloride.
3. The perovskite solar cell according to claim 1, characterized in that The interface modification layer is prepared by the following steps: dynamically spin-coating an organic hydrochloride molecule solution onto the surface of a perovskite light-absorbing layer to obtain the interface modification layer; the solvent of the organic hydrochloride molecule solution is isopropanol, and the concentration of the solution is 0.1-1.5 mg / mL.
4. The perovskite solar cell according to claim 3, characterized in that: The conditions of the dynamic spin coating are: a spin coating speed of 3000 to 7000 rpm and a spin coating time of 20 to 60 s.
5. The perovskite solar cell according to any one of claims 1 to 4, characterized in that: The thickness of the interface modification layer is 2-10 nm.
6. The perovskite solar cell according to claim 1 or 2, characterized in that: The transparent conductive substrate is selected from one of ITO conductive glass, FTO conductive glass and transparent conductive flexible plastic.
7. The perovskite solar cell according to claim 1 or 2, characterized in that: The material of the hole transport layer is one or more of nickel oxide, 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-diphenyl-9H-carbazole-9-yl)ethyl]phosphonic acid and (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid, or a stacked material formed by the above materials.
8. The perovskite solar cell according to claim 1 or 2, characterized in that: The material of the perovskite light absorbing layer is metal halide perovskite, the crystal structure of the metal halide perovskite is ABX3, A is selected from at least one of organic cations and inorganic cations, B is selected from divalent metal ions, and X is selected from halogen ions; the material of the electron transport layer is selected from PCBM, C 60 One of them.
9. The perovskite solar cell according to claim 1 or 2, characterized in that: The material of the hole blocking layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline; the material of the electrode layer is selected from one of aluminum, silver and copper.
10. The method for preparing an interface-modified perovskite solar cell according to claim 1 or 2, characterized in that: The steps include: S1. Preparing a hole transport layer on the surface of a transparent conductive substrate by vacuum deposition or solution deposition; S2, preparing a perovskite light absorbing layer by coating the surface of the hole transport layer; S3, preparing an interface modification layer on the surface of the perovskite light-absorbing layer by dynamically spin-coating an organic hydrochloride molecular solution; S4, preparing an electron transport layer on the surface of the interface modification layer by vacuum deposition or solution deposition; S5, preparing a hole blocking layer on the surface of the electron transport layer by vacuum deposition or solution deposition; S6. Prepare an electrode layer on the surface of the hole blocking layer by evaporation method to obtain the perovskite solar cell.
Citation Information
Cited By
Perovskite solar cell and preparation method and application thereof
CN120018683A
Ditrimethoprim hydrochloride modified inverted inorganic perovskite solar cell and preparation thereof
CN122121402A
Trimethoprim hydrochloride modified inverted inorganic perovskite solar cell and preparation thereof
CN122121402B