Fluorine-containing polymer, preparation method, insulating coating layer, secondary battery and electric device

CN118765290APending Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202280092948.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing insulating coating has a short process window and poor fluidity, which results in low production efficiency of battery pole pieces. It is easy for precipitation to block the pipeline and affect the quality of the pole pieces.

Method used

Fluoropolymer is used as the binder and is prepared through polymerization reaction to improve the filterability and fluidity of the slurry, broaden the process window, enhance the bonding force, and reduce the dependence on the dispersant.

Benefits of technology

It significantly improves the production efficiency and quality of insulating coatings, ensures that the slurry does not gel after standing, enhances adhesion and processing performance, and is suitable for insulating coating applications in secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765290A_ABST
    Figure CN118765290A_ABST
Patent Text Reader

Abstract

The invention relates to # imgabs0, a fluorine-containing polymer, a preparation method, an insulating coating, a secondary battery and an electric device. The fluorine-containing polymer comprises a structural unit derived from a monomer as shown in a formula I, a structural unit derived from an olefin monomer and a structural unit derived from a monomer as shown in a formula II; based on the total mole number of the structural units in the fluorine-containing polymer, the mole content of the structural units derived from the monomer shown in the formula I is 60-80%. Wherein R1, R2 and R3 are respectively and independently selected from hydrogen, fluorine, chlorine or C1-3 alkyl containing at least one fluorine atom, and R4, R5 and R6 are respectively and independently selected from hydrogen or substituted or unsubstituted C1-5 alkyl.
Need to check novelty before this filing date? Find Prior Art

Description

Fluoropolymer, preparation method, insulating coating, secondary battery, and electrical device Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a fluorine-containing polymer, a preparation method, an insulating coating, a secondary battery, and an electrical device. Background Art

[0002] During the production process of battery cell electrodes, an insulating coating is applied to the current collector surface to prevent the positive and negative electrodes from short-circuiting during use, potentially leading to safety incidents and even fires and explosions. This insulating coating is typically applied to the current collector surface using an insulating slurry composed of a binder, inorganic insulating materials, and additives. However, existing insulating slurries have a short processing window, poor fluidity, and are prone to precipitation and clogging pipelines, severely impacting electrode production efficiency. Therefore, the development of a binder to improve the slurry's processing properties is urgently needed.

[0003] Summary of the Invention

[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a fluoropolymer and an insulating coating comprising the fluoropolymer, so as to optimize the process window for preparing the insulating coating and improve the production efficiency of the insulating coating.

[0005] The first aspect of the present application provides a fluoropolymer comprising a structural unit derived from a monomer represented by formula I, a structural unit derived from an olefin monomer, and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of the structural units in the fluoropolymer.

[0006]

[0007] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 alkyl.

[0008] The fluoropolymer provided in the present application can improve the filterability and fluidity of the slurry, so that the slurry does not gel after standing for 6 hours, significantly broadens the process window of the slurry, improves the processability of the slurry, and enables the slurry to meet the production requirements of the insulating coating without adding a dispersant, which is beneficial to optimizing the production process of the insulating coating and improving its production efficiency.

[0009] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

[0010] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula II is 5% to 25%, based on the total molar number of all structural units in the fluorine-containing polymer.

[0011] Based on the total molar number of all structural units in the fluoropolymer, when the molar content of the structural unit derived from the monomer represented by Formula II is 5% to 25%, the fluoropolymer further improves the fluidity and filterability of the insulating slurry, further broadens the process window for insulating slurry processing, and the fluoropolymer enables the insulating coating to have effective adhesion.

[0012] In any embodiment, the molar content of the structural unit derived from the olefin monomer is 5% to 30%, based on the total moles of all structural units in the fluorine-containing polymer.

[0013] Based on the total molar number of all structural units in the fluoropolymer, when the molar content derived from olefin monomers is 5% to 30%, the fluoropolymer further improves the fluidity and filterability of the insulating slurry, further broadens the process window for insulating slurry processing, and the fluoropolymer enables the insulating coating to have effective adhesion.

[0014] In any embodiment, the weight average molecular weight of the fluorine-containing polymer is 500,000 to 800,000.

[0015] Fluoropolymers with a weight-average molecular weight between 500,000 and 800,000 are beneficial to further improving the fluidity and filterability of the insulating slurry, further broadening the process window for insulating slurry processing, and helping the insulating coating maintain effective adhesion.

[0016] In any embodiment, the viscosity of the adhesive prepared by dissolving the fluorine-containing polymer in N-methylpyrrolidone is 1000-3000 mPa·s, and the mass content of the fluorine-containing polymer in the adhesive is 7%, based on the total mass of the adhesive.

[0017] The viscosity of the adhesive containing 7% by mass of the fluoropolymer prepared by dissolving the fluoropolymer in N-methylpyrrolidone is 1000-3000 mPa·s. This means that the insulating paste using the fluoropolymer as a binder does not require the addition of additional additives, effectively optimizing the production process and improving production efficiency, while also facilitating improved batch stability of the insulating coating.

[0018] In any embodiment, the monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0019] In any embodiment, the olefin monomer is selected from one or more of propylene, 2-butene, and butadiene.

[0020] In any embodiment, the monomer represented by formula II is selected from one or both of acrylic acid and methacrylic acid.

[0021] A second aspect of the present application provides a method for preparing a fluorinated polymer, comprising the following steps:

[0022] A fluorine-containing polymer is prepared by polymerizing at least one monomer represented by formula I, at least one olefin monomer, and at least one monomer represented by formula II under polymerizable conditions, wherein the molar content of the monomer represented by formula I is 60% to 80%, based on the total molar number of the monomer represented by formula I, the olefin monomer, and the monomer represented by formula II.

[0023]

[0024] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 In the alkyl group, R4, R5, and R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 alkyl.

[0025] Compared with traditional binders, the fluoropolymer prepared by this method can improve the filterability and fluidity of the slurry, so that the slurry does not gel after standing for 6 hours, significantly broadens the process window of the slurry, improves the processability of the slurry, and enables the slurry to meet the production requirements of the insulating coating without adding a dispersant, which is conducive to optimizing the production process of the insulating coating and improving its production efficiency.

[0026] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

[0027] In any embodiment, the polymerization reaction comprises the following steps:

[0028] First stage polymerization: providing a first initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to start the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;

[0029] Second stage polymerization: After a period of reaction, olefin monomer and monomer represented by formula II are fed into the reaction vessel for second stage polymerization; when the pressure in the reaction vessel drops to less than or equal to 0.5 MPa, the reaction is stopped, solid-liquid separation is performed, and the solid phase is retained.

[0030] The method provided by the present application first continuously feeds the monomer shown in formula I to form a fluorine-containing segment, so that the fluorine-containing polymer has high thermal stability; then the monomer shown in formula II and the olefin monomer are introduced to reduce the contact of the fluorine-containing segment with the external environment, effectively alleviating the gelation phenomenon caused by the fluorine element. The fluorine-containing polymer prepared by this method can more effectively improve the filterability and fluidity of the insulating slurry than the fluorine-containing polymer prepared by simultaneously polymerizing all the monomers into the reaction vessel, further broaden the process window of the slurry, and help improve the production efficiency of the insulating coating.

[0031] In any embodiment, the initial reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 70° C. to 90° C.

[0032] In any embodiment, the second stage polymerization comprises the following steps:

[0033] When the mass of the monomer represented by formula I fed in is 70% to 85% of the total mass of the monomer represented by formula I supplied during the polymerization reaction, a mixed gas of the monomer represented by formula I and an olefin monomer is fed into the reaction vessel, and the initial reaction pressure is maintained to continue the reaction;

[0034] After all the monomers represented by formula I are fed into the reaction container, a mixture of olefin monomers and monomers represented by formula II is fed into the reaction container.

[0035] Before feeding the monomer represented by formula II into the reaction vessel, a mixed gas of the monomer represented by formula I and an olefin monomer is first fed into the reaction vessel. Using the olefin monomer as a bridge helps to overcome the problems of large reaction differences and poor compatibility between the monomer represented by formula I and the monomer represented by formula II, thereby improving the degree of polymerization of the fluorine-containing polymer.

[0036] In any embodiment, the ratio of the total moles of olefin monomers supplied during the polymerization reaction to the total moles of the monomers represented by formula I is 1:16-1:2.

[0037] In any embodiment, the ratio of the total moles of olefin monomers supplied during the polymerization reaction to the total moles of the monomers represented by formula I is 1:16-1:3.

[0038] In any embodiment, in the mixed gas, the molar ratio of the olefin monomer to the monomer represented by formula I is 1:1-2:1.

[0039] In any embodiment, in the mixture, the molar ratio of the olefin monomer to the monomer represented by formula II is 3:1-4:1.

[0040] In any embodiment, the second stage polymerization further comprises the following steps:

[0041] Before feeding the mixed gas of the monomer represented by Formula I and the olefin monomer into the reaction container, the first initiator and the second initiator are added into the reaction container.

[0042] In any embodiment, the second stage polymerization further comprises the following steps:

[0043] Before feeding the mixture of olefin monomer and monomer represented by formula II into the reaction container, a second initiator is added into the reaction container.

[0044] In any embodiment, the first initiator is a persulfate, which can be selected from one or more of potassium persulfate and ammonium persulfate.

[0045] In any embodiment, the second initiator is a thiosulfate salt, which can be selected from sodium thiosulfate.

[0046] The third aspect of the present application provides an application of the fluorine-containing polymer of the first aspect in a secondary battery. Optionally, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.

[0047] A fourth aspect of the present application provides an insulating coating comprising a binder and an inorganic insulating material, wherein the binder is the fluorine-containing polymer of the first aspect.

[0048] The insulating coating is easy to process and prepare and has good uniformity, which helps to improve battery production capacity.

[0049] In any embodiment, the binder has a mass content of 7.0% to 13.0%, based on the total mass of the insulating coating.

[0050] When the mass content of the binder is 7.0%-13.0% of the total mass of the insulating coating, the binder further improves the fluidity and filterability of the insulating slurry, further broadens the process window for insulating slurry processing, and the binder can ensure that the insulating coating maintains effective bonding.

[0051] In any embodiment, the inorganic insulating material comprises a colored oxide, which may be selected from black zirconium dioxide, yellow zirconium dioxide, red zirconium dioxide, or green zirconium dioxide.

[0052] The applicant unexpectedly discovered that including colored oxides in the insulating coating helps to improve the laser cutting quality and laser cutting speed of the pole piece.

[0053] In any embodiment, the mass content of the colored oxide is 0.2%-3%, based on the total mass of the insulating coating.

[0054] When the mass content of the colored oxide in the insulating coating is 0.2%-3%, it helps to improve the laser cutting performance with maximum efficiency.

[0055] A fifth aspect of the present application provides a method for preparing an insulating coating, comprising the following steps:

[0056] Dispersing a binder in a solvent to prepare a glue solution, wherein the binder is the fluorine-containing polymer of the first aspect of the present application;

[0057] Mixing the inorganic insulating material with the glue and stirring to prepare a slurry, wherein the solid content of the slurry is 30%-40%;

[0058] The slurry is coated on a current collector to prepare an insulating coating.

[0059] The insulating coating prepared by the method has high efficiency and uniform quality.

[0060] In any embodiment, when the solid content of the slurry is 30%-40%, the viscosity of the slurry is 2500-4000 mPa·s.

[0061] The viscosity of the slurry with a solid content of 30%-40% is 2500-4000mPa·s, and it can be directly used for production coating without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.

[0062] In any embodiment, the mixing of the inorganic insulating material and the glue comprises the following steps:

[0063] The inorganic insulating material except the colored oxide is mixed with the glue, stirred, and then the colored oxide is added and stirred again to prepare the slurry.

[0064] Adding colored oxides in the final stage of the slurry preparation process is beneficial to improving the color uniformity of the prepared insulating coating and is beneficial to improving the subsequent laser cutting speed and laser cutting quality.

[0065] The sixth aspect of the present application provides a secondary battery, comprising a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet comprises the insulating coating of the fourth aspect of the present application; optionally, the secondary battery comprises at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery and a potassium ion battery.

[0066] A seventh aspect of the present application provides a battery module including the secondary battery according to the sixth aspect of the present application.

[0067] An eighth aspect of the present application provides a battery pack comprising the secondary battery of the sixth aspect of the present application or the battery module of the seventh aspect of the present application.

[0068] The ninth aspect of the present application provides an electrical device comprising at least one selected from the secondary battery of the sixth aspect of the present application, the battery module of the seventh aspect of the present application, or the battery pack of the eighth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] FIG1 is a schematic diagram of a pole piece including an insulating coating;

[0070] FIG2 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0071] FIG3 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG2 ;

[0072] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application;

[0073] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0074] FIG6 is an exploded view of the battery pack shown in FIG5 according to an embodiment of the present application;

[0075] 7 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application;

[0076] FIG8 is a microscope image of the pole piece after laser cutting of Example 26 of the present application, (A) is a plan view of the pole piece cut, and (B) is a cross-sectional view of the pole piece cut;

[0077] Figure 9 is a microscope image of the pole piece after laser cutting of Example 6 of the present application, (A) is a plan view of the pole piece cut, and (B) is a cross-sectional view of the pole piece cut.

[0078] Description of reference numerals:

[0079] 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 cover; 6 pole piece; 61 current collector; 62 active material layer; 63 insulating coating. DETAILED DESCRIPTION

[0080] Below, the embodiments of the binder, preparation method, electrode, battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0081] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0082] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0083] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0084] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0085] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0086] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0087] Safety is one of the most important research topics in secondary batteries. As shown in Figure 1, during the preparation process, an insulating coating 63 is applied between the current collector 61 used to form the tab and the active material layer 62 of the electrode 6 to prevent direct contact between the positive and negative electrodes during use of the battery cell, resulting in a short circuit, which could cause a safety accident or even lead to a fire or explosion. Due to the high electrical resistance of inorganic materials, inorganic materials are often dispersed in a binder to form a slurry to prepare the insulating coating. However, traditional binders have excessive viscosity and are prone to slurry precipitation, resulting in poor slurry uniformity and large performance variance between batches of the insulating coating. Furthermore, traditional binders can make the slurry less fluid and difficult to apply evenly. Therefore, a dispersant needs to be added during the slurry preparation process to improve the slurry's processing properties. This undoubtedly increases the difficulty of slurry processing, affects production efficiency, and leads to poor slurry stability between batches. Based on the above technical problems, the present application has developed a binder that gives the slurry better fluidity and filterability to improve the production efficiency and quality of the insulating coating.

[0088] Based on this, the present application proposes a fluoropolymer comprising a structural unit derived from a monomer represented by formula I, a structural unit derived from an olefin monomer, and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of the structural units in the fluoropolymer.

[0089]

[0090] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 alkyl.

[0091] As used herein, the term "fluoropolymer" refers to a polymer containing fluorine in its structural units.

[0092] As used herein, the term "polymer" includes, on the one hand, a collection of chemically homogeneous macromolecules prepared by polymerization, but differing in degree of polymerization, molar mass, and chain length. The term also includes derivatives of such collections of macromolecules formed by polymerization, i.e., products that can be obtained by reaction of functional groups in the aforementioned macromolecules, such as addition or substitution, and can be chemically homogeneous or chemically heterogeneous.

[0093] In this article, the term “C 1-5 "Alkyl" refers to a straight or branched hydrocarbon chain radical consisting solely of carbon and hydrogen atoms, with no unsaturation present, having from one to five carbon atoms, and attached to the remainder of the molecule by a single bond. 1-3 "Alkyl" should be interpreted accordingly. C 1-5 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, 1-methylethyl (isopropyl), butyl, and pentyl. In some embodiments, C 1-3 Alkyl is -CF3, -CH3CH2F or -CH2FCH2F.

[0094] As used herein, the term "substituted" refers to a compound or chemical moiety in which at least one hydrogen atom is replaced by another chemical moiety, wherein the substituents are each independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.

[0095] As used herein, the term "olefin monomer" refers to a hydrocarbon containing at least one C=C bond (carbon-carbon double bond). Examples of olefin monomers include, but are not limited to, ethylene, propylene, butene, and butadiene. In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or both of hydrogen and methyl.

[0096] In some embodiments, the fluoropolymer includes at least two structural units derived from different monomers of Formula I, one of which is derived from vinylidene fluoride. The different monomer types help reduce the ordered arrangement of the fluoropolymer long chains, reduce crystallinity, and increase flexibility.

[0097] In some embodiments, the monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0098] In some embodiments, the olefin monomer is selected from one or more of propylene, 2-butene, and butadiene.

[0099] In some embodiments, the monomer represented by Formula II is selected from one or both of acrylic acid and methacrylic acid.

[0100] In some embodiments, the polymer comprises one or more structural units derived from the monomers of formula I. In some embodiments, the polymer comprises one or more structural units derived from the monomers of formula II. In some embodiments, the polymer includes but is not limited to vinylidene fluoride-ethylene-acrylic acid copolymer, vinylidene fluoride-butadiene-acrylic acid copolymer, vinylidene fluoride-propylene-acrylic acid copolymer, vinylidene fluoride-ethylene-methacrylic acid copolymer, vinylidene fluoride-hexafluoropropylene-ethylene-acrylic acid copolymer, vinylidene fluoride-hexafluoropropylene-ethylene-methacrylic acid copolymer, and vinylidene fluoride-chlorotrifluoroethylene-butadiene-methacrylic acid copolymer.

[0101] In some embodiments, the molar content of the structural units derived from the monomer represented by Formula I can be 60%, 65%, 70%, 75% or 80%, based on the total moles of the structural units in the fluoropolymer.

[0102] The fluorine element in the structural unit derived from the monomer shown in formula I can form hydrogen bonds with the hydroxyl and / or carboxyl groups on the surface of the current collector, so that the insulating coating has good adhesion and is not easy to fall off during the manufacturing and use process, causing safety accidents. The structural unit derived from the olefin monomer and the monomer shown in formula II can effectively reduce the fluorine content of the fluorine-containing polymer, so that the molar content of the structural unit derived from the monomer shown in formula I is 60%-80%, which can improve the slurry gel phenomenon caused by the fluorine element. Moreover, the structural unit derived from the olefin monomer and the monomer shown in formula II can further increase the steric hindrance of the fluorine-containing polymer, reduce the aggregation of the fluorine-containing units, stabilize the slurry, alleviate the sedimentation of the slurry, and effectively improve the filterability of the slurry.

[0103] Compared with traditional binders, the fluoropolymer provided in the present application can improve the filterability and fluidity of the slurry, so that the slurry does not gel after standing for 6 hours, significantly broadens the process window of the slurry, improves the processability of the slurry, and enables the slurry to meet the production requirements of the insulating coating without adding a dispersant, which is beneficial to optimizing the production process of the insulating coating and improving its production efficiency.

[0104] In this article, the term "process window" refers to the process range that can ensure product quality, including but not limited to temperature range, pressure range, storage time length, etc. It can be understood that the wider the process window, the lower the requirement for process accuracy.

[0105] In some embodiments, the molar content of the structural unit derived from the monomer of Formula II is 5% to 25%, based on the total moles of all structural units in the fluoropolymer. In some embodiments, the molar content of the structural unit derived from the monomer of Formula II can be any one of 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, and 25%, based on the total moles of all structural units in the fluoropolymer.

[0106] Based on the total molar number of all structural units in the fluoropolymer, when the molar content of the structural unit derived from the monomer represented by Formula II is 5% to 25%, on the one hand, the appropriate content of polar carboxyl groups will not cause gelation of the slurry, thereby further improving the fluidity and filterability of the insulating slurry and further broadening the process window for insulating slurry processing; on the other hand, the appropriate content of carboxyl groups enables the insulating coating to maintain effective adhesion.

[0107] In some embodiments, the molar content of the structural units derived from olefin monomers is 5% to 30%, based on the total moles of all structural units in the fluoropolymer. In some embodiments, the molar content of the structural units derived from olefin monomers can be any one of 5%, 10%, 15%, 20%, 25%, and 30%, based on the total moles of all structural units in the fluoropolymer.

[0108] Based on the total molar number of all structural units in the fluoropolymer, when the molar content derived from olefin monomers is 5% to 30%, the fluoropolymer further improves the fluidity and filterability of the insulating slurry, further broadens the process window for insulating slurry processing, and the fluoropolymer enables the insulating coating to maintain effective adhesion.

[0109] In some embodiments, the weight average molecular weight of the fluorine-containing polymer is 500,000-800,000. In some embodiments, the weight average molecular weight of the fluorine-containing polymer can be any one of 500,000, 600,000, 650,000, 700,000, 750,000, and 800,000.

[0110] As used herein, the term "weight average molecular weight" refers to the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights.

[0111] In the present application, the weight-average molecular weight of the polymer can be tested using methods known in the art, such as gel chromatography, such as using a Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141). In some embodiments, the testing method is to use a polystyrene solution sample with a mass fraction of 3.0% as a reference and select a matching chromatographic column (oily: Styragel HT5DMF7.8*300mm+Styragel HT4). Use purified N-methylpyrrolidone (NMP) solvent to prepare a 3.0% fluoropolymer glue, and let the prepared solution stand for one day for use. During the test, first use a syringe to draw tetrahydrofuran, rinse, and repeat several times. Then draw 5 ml of the experimental solution, expel the air in the syringe, and wipe the needle tip dry. Finally, slowly inject the sample solution into the injection port. After the reading stabilizes, obtain the data and read the weight-average molecular weight.

[0112] Fluoropolymers with a weight-average molecular weight between 500,000 and 800,000 give the adhesive a suitable viscosity, which is beneficial to further improve the fluidity and filterability of the insulating slurry and further broaden the process window for insulating slurry processing; at the same time, fluoropolymers with a suitable weight-average molecular weight are conducive to forming a three-dimensional network bonding structure, which helps the insulating coating maintain effective bonding.

[0113] In some embodiments, the viscosity of the glue obtained by dissolving the fluoropolymer in N-methylpyrrolidone is 1000-3000 mPa·s, and the mass content of the fluoropolymer in the glue is 7%, based on the total mass of the glue. In some embodiments, the viscosity of the glue obtained by dissolving the fluoropolymer in N-methylpyrrolidone can be any one of 1000 mPa·s, 1500 mPa·s, 2000 mPa·s, 2500 mPa·s, and 3000 mPa·s, and the mass content of the fluoropolymer in the glue is 7%, based on the total mass of the glue.

[0114] In the present application, the viscosity of the fluorine-containing polymer glue can be tested by methods known in the art, such as using a rotary viscometer for testing.

[0115] The adhesive solution, prepared by dissolving a fluoropolymer in N-methylpyrrolidone, has a viscosity of 1000-3000 mPa·s. The fluoropolymer content in the adhesive solution is 7% by weight, based on the total weight of the adhesive solution. This eliminates the need for additional additives in insulating pastes using this fluoropolymer as a binder, effectively optimizing the production process and improving production efficiency. Furthermore, the adhesive solution within this viscosity range combines fluidity and viscosity, enhancing the adhesion of the insulating coating while ensuring uniform coating application, which contributes to improved batch stability of the insulating coating.

[0116] In one embodiment of the present application, a method for preparing a fluorine-containing polymer is provided, comprising the following steps:

[0117] A fluorine-containing polymer is prepared by polymerizing at least one monomer represented by formula I, at least one olefin monomer, and at least one monomer represented by formula II under polymerizable conditions, wherein the molar content of the monomer represented by formula I is 60% to 80%, based on the total moles of the monomer represented by formula I, the olefin monomer, and the monomer represented by formula II.

[0118]

[0119] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 alkyl.

[0120] As used herein, the term "polymerizable conditions" refers to those conditions including temperature, pressure, reactant concentrations, optional solvents / diluents, reactant mixing / addition parameters selected by one skilled in the art, and other conditions that facilitate the reaction of one or more monomers within at least one polymerization reactor.

[0121] Compared with traditional binders, the fluoropolymer prepared by this method can improve the filterability and fluidity of the slurry, so that the slurry does not gel after standing for 6 hours, significantly broadens the process window of the slurry, improves the processability of the slurry, and enables the slurry to meet the production requirements of the insulating coating without adding a dispersant, which is conducive to optimizing the production process of the insulating coating and improving its production efficiency.

[0122] In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

[0123] In some embodiments, at least two monomers of Formula I are added during the polymer preparation process, wherein one monomer of Formula I is polyvinylidene fluoride. The addition of different monomers helps to reduce the order of the long chains of the fluoropolymer, reduce the crystallinity, and improve the flexibility of the fluoropolymer.

[0124] In some embodiments, the polymerization reaction comprises the following steps:

[0125] First stage polymerization: providing a first initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;

[0126] Second stage polymerization: After a period of reaction, olefin monomer and monomer represented by formula II are fed into the reaction vessel for second stage polymerization; when the pressure in the reaction vessel drops to less than or equal to 0.5 MPa, the reaction is stopped, solid-liquid separation is performed, and the solid phase is retained.

[0127] As used herein, the term "continuous feeding" refers to the slow, small, incremental addition of monomers.

[0128] In some embodiments, the first initiator is a persulfate, which can be selected from one or more of potassium persulfate and ammonium persulfate. Potassium persulfate effectively decomposes above 60°C to generate free radical ions or ionic free radicals, which are suitable as an initiator for emulsion polymerization.

[0129] In some embodiments, the emulsifier is an alkali metal perfluorooctanoate, optionally a sodium perfluorooctanoate.

[0130] In some embodiments, the solvent is an aqueous solvent, which may be deionized water.

[0131] The method provided by the present application first continuously feeds the monomer shown in formula I to form a fluorine-containing segment, so that the fluorine-containing polymer has high thermal stability; then the monomer shown in formula II and the olefin monomer are introduced to reduce the contact of the fluorine-containing segment with the external environment, effectively alleviating the gelation phenomenon caused by the fluorine element. The fluorine-containing polymer prepared by this method can more effectively improve the filterability and fluidity of the slurry than the fluorine-containing polymer prepared by simultaneously polymerizing all the monomers into the reaction vessel, further broaden the process window of the slurry, and help improve the production efficiency of the insulating coating.

[0132] In some embodiments, the initial reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 70° C. to 90° C.

[0133] In some embodiments, the second stage polymerization comprises the following steps:

[0134] When the mass of the monomer represented by formula I fed in is 70% to 85% of the total mass of the monomer represented by formula I supplied during the polymerization reaction, a mixed gas of the monomer represented by formula I and an olefin monomer is fed into the reaction vessel, and the initial reaction pressure is maintained to continue the reaction;

[0135] After all the monomers represented by formula I are fed into the reaction container, a mixture of olefin monomers and monomers represented by formula II is fed into the reaction container.

[0136] Before feeding the monomer represented by formula II into the reaction vessel, a mixed gas of the monomer represented by formula I and an olefin monomer is first fed into the reaction vessel. Using the olefin monomer as a bridge helps to overcome the problems of large reaction differences and poor compatibility between the monomer represented by formula I and the monomer represented by formula II, thereby improving the degree of polymerization of the fluorine-containing polymer.

[0137] In some embodiments, the ratio of the total moles of olefin monomers supplied during the polymerization reaction to the total moles of the monomers represented by Formula I is 1:16 to 1:2.

[0138] In some embodiments, the ratio of the total moles of the monomers of Formula II supplied during the polymerization reaction to the total moles of the monomers of Formula I is 1:16-1:3.

[0139] In some embodiments, the molar ratio of the olefin monomer to the monomer represented by Formula I in the mixed gas is 1:1-2:1.

[0140] In some embodiments, in the mixture, the molar ratio of the olefin monomer to the monomer represented by Formula II is 3:1-4:1.

[0141] In some embodiments, the second stage polymerization further comprises the following steps:

[0142] Before feeding the mixed gas of the monomer represented by Formula I and the olefin monomer into the reaction container, the first initiator and the second initiator are added into the reaction container.

[0143] In some embodiments, the second initiator is a thiosulfate, which can be selected from sodium thiosulfate. As a reducing agent, the thiosulfate easily reacts with the first initiator persulfate in the reaction vessel to generate two free radicals, effectively initiating the polymerization of the olefin monomer.

[0144] In some embodiments, the second stage polymerization further comprises the following steps:

[0145] Before feeding the mixture of olefin monomer and monomer represented by formula II into the reaction container, a second initiator is added into the reaction container.

[0146] In one embodiment of the present application, a fluoropolymer according to any embodiment is provided for use in a secondary battery. Optionally, the secondary battery comprises at least one of a lithium-ion battery, a sodium-ion battery, a magnesium-ion battery, and a potassium-ion battery. In some embodiments, the fluoropolymer is used as a binder in a secondary battery. In some embodiments, the fluoropolymer is used as a binder for an insulating coating in a secondary battery.

[0147] [Insulation coating]

[0148] In one embodiment of the present application, an insulating coating is provided, comprising a binder and an inorganic insulating material, wherein the binder is a fluorine-containing polymer in any embodiment.

[0149] As used herein, the term "binder" refers to a chemical compound, polymer, or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.

[0150] In this application, the term "inorganic insulating material" refers to a material with a resistivity greater than 10 6 Ω·cm inorganic materials and their precursors include but are not limited to boehmite, barium carbonate, barium sulfate, aluminum oxide, zirconium dioxide, calcium carbonate, and silicon dioxide.

[0151] In some embodiments, the inorganic insulating material includes boehmite. Boehmite (AlOOH), a precursor of γ-Al2O3, has excellent adhesion to the current collector, making it less susceptible to detachment as an insulating coating. In some embodiments, the inorganic insulating material includes zirconium dioxide. Zirconium dioxide has high electrical resistivity and is suitable for forming an insulating coating.

[0152] In some embodiments, the dispersion medium of the binder is an aqueous solvent, such as deionized water, that is, the binder is dissolved in the aqueous solvent.

[0153] In some embodiments, the binder dispersion medium is an oily solvent. Examples of such oily solvents include, but are not limited to, dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, acetone, dimethyl carbonate, ethyl cellulose, and polycarbonate. That is, the binder is dissolved in the oily solvent.

[0154] In some embodiments, a binder is used to hold the inorganic insulating materials in place and adhere them to the current collector to form an insulating coating.

[0155] The insulating coating is easy to process and prepare and has good uniformity, which helps to improve battery production capacity.

[0156] In some embodiments, the binder content is 7.0% to 13.0% by weight, based on the total weight of the insulating coating. In some embodiments, the binder content is any one of 7.0%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, and 13.0% by weight, based on the total weight of the insulating coating.

[0157] When the mass content of the binder is 7.0%-13.0% of the total mass of the insulating coating, the insulating slurry has a suitable viscosity, which further improves the fluidity and filterability of the insulating slurry and further broadens the process window for insulating slurry processing; at the same time, the mass content of the binder in the appropriate range ensures that the insulating coating and the current collector have sufficient bonding force.

[0158] In some embodiments, the inorganic insulating material comprises a colored oxide, which can be selected from one or more of black zirconium dioxide, yellow zirconium dioxide, red zirconium dioxide, and green zirconium dioxide. In some embodiments, the colored oxide is colored zirconium dioxide. In some embodiments, the inorganic insulating material comprises black zirconium dioxide.

[0159] The applicant unexpectedly discovered that the inclusion of colored oxides in the insulating coating can help improve the laser cutting quality and laser cutting speed of the pole piece. Laser cutting refers to the technology of processing the material by irradiating the workpiece with a focused high-power density laser beam to rapidly heat, melt, vaporize, ablate or decompose the irradiated material. The application of laser cutting technology in secondary batteries mainly includes laser pole piece cutting, tab cutting and diaphragm cutting. At present, there are problems such as many burrs in the cutting area and limited maximum cutting speed in laser cutting of pole pieces. In the prior art, inorganic insulating materials are generally colorless or white powders. The applicant found that the inclusion of colored oxides in inorganic insulating materials can increase the maximum cutting speed of pole pieces by more than 30%, which helps to significantly increase battery production capacity. At the same time, the colored oxides in the inorganic insulating material can reduce the heat-affected zone of the laser, improve cutting quality, reduce cutting burrs, and reduce the impact of the processing process on battery performance.

[0160] In some embodiments, the mass content of the colored oxide is 0.2% to 3%, based on the total mass of the insulating coating.

[0161] When the mass content of colored oxides in the insulating coating is 0.2%-3%, it can not only improve the cutting speed during the laser cutting and forming process of the pole piece, but also take into account the raw material cost, which helps to maximize the efficiency of laser cutting performance.

[0162] In some embodiments, the colored oxide is black zirconium oxide. When the colored oxide accounts for more than 3.0% by mass of the insulating coating, there is no color difference between the insulating coating and the active material layer, making it difficult for the laser cutting system to identify and locate them, which is not conducive to accurate cutting.

[0163] In one embodiment of the present application, a method for preparing an insulating coating is provided, comprising the following steps:

[0164] Dispersing a binder in a solvent to prepare a glue solution, wherein the binder is a fluorine-containing polymer in any embodiment;

[0165] Mix the inorganic insulating material and the glue, stir and prepare a slurry, the solid content of the slurry is 30%-40%;

[0166] The slurry is coated on a current collector to prepare an insulating coating.

[0167] The solid content of the slurry is 30% to 40%. On the one hand, it makes the slurry have a suitable viscosity, which is beneficial to the subsequent coating and drying work; on the other hand, the suitable slurry viscosity can improve the stability of the slurry and facilitate the preservation of the slurry.

[0168] The insulating coating prepared by the above method has high efficiency and does not require the addition of other additives, which is beneficial to saving production processes and improving production efficiency.

[0169] In some embodiments, the slurry has a viscosity of 2500-4000 mPa·s at a solid content of 30%-40%. In some embodiments, the viscosity of the slurry at a solid content of 30%-40% can be any one of 2750 mPa·s, 3000 mPa·s, 3250 mPa·s, 3500 mPa·s, 3750 mPa·s, and 4000 mPa·s.

[0170] The viscosity of the slurry with a solid content of 30%-40% is 2500-4000mPa·s, and it can be directly used for production coating without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.

[0171] In some embodiments, mixing the inorganic insulating material with the glue comprises the following steps:

[0172] The inorganic insulating material except the colored oxide is mixed with the glue, stirred, and then the colored oxide is added and stirred again to prepare the slurry.

[0173] Adding colored oxides in the final stage of the slurry preparation process is beneficial to improving the color uniformity of the prepared insulating coating and improving the subsequent laser cutting speed and quality.

[0174] In one embodiment of the present application, a secondary battery is provided, comprising a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet include the insulating coating described in any embodiment. In some embodiments, the secondary battery comprises at least one of a lithium-ion battery, a sodium-ion battery, a magnesium-ion battery, and a potassium-ion battery. During the charge and discharge process of the battery, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0175] [Positive electrode]

[0176] The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer and an insulating coating layer disposed on at least one surface of the positive electrode current collector.

[0177] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer and the insulating coating layer are provided on either or both of the two facing surfaces of the positive electrode current collector.

[0178] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0179] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0180] In some embodiments, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0181] In some embodiments, the positive electrode active material layer may further optionally include: As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0182] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode active material layer, such as the positive electrode active material, the conductive agent, the binder, and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing, etc., the positive electrode active material layer is obtained. The components for preparing the insulating coating, such as the fluoropolymer, are dispersed in a solvent (such as N-methylpyrrolidone) to form a glue; the inorganic insulating material and the glue are mixed and stirred to prepare an insulating slurry; the insulating slurry is coated on the positive electrode current collector along the edge of the positive electrode active material layer, and after drying, cold pressing, etc., the insulating coating is obtained. The positive electrode sheet is obtained by using the same method on the other side of the current collector to obtain the positive electrode active material layer and the insulating coating.

[0183] [Negative electrode]

[0184] The negative electrode sheet includes a negative electrode current collector, a negative electrode active material layer and an insulating coating layer disposed on at least one surface of the negative electrode current collector.

[0185] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0186] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0187] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0188] In some embodiments, the negative electrode active material layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0189] In some embodiments, the negative electrode active material layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0190] In some embodiments, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0191] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode active material layer, such as the negative electrode active material, conductive agent, binder, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing, and other processes, the negative electrode active material layer is obtained. The components for preparing the insulating coating, such as the fluoropolymer, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a glue; the inorganic insulating material and the glue are mixed and stirred to prepare an insulating slurry; the insulating slurry is coated on the negative electrode current collector along the edge of the negative electrode active material layer, and after drying, cold pressing, and other processes, the insulating coating is obtained. The negative electrode sheet is obtained by using the same method to obtain the negative electrode active material layer and insulating coating on the other side of the negative electrode current collector.

[0192] [Electrolytes]

[0193] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0194] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0195] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0196] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0197] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0198] [Isolation film]

[0199] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0200] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0201] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0202] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0203] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0204] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a secondary battery 5 having a square structure as an example.

[0205] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0206] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0207] Figure 4 shows an example battery module 4. Referring to Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0208] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0209] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0210] Figures 5 and 6 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0211] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0212] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0213] Figure 7 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0214] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0215] Example

[0216] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0217] 1. Preparation method

[0218] Example 1

[0219] 1) Preparation of binder (fluoropolymer)

[0220] 30 kg of deionized water (conductivity less than or equal to 2 μs / cm), 21 g of sodium perfluorooctanoate, and 71.4 g of 5% potassium persulfate solution were added to the reactor in sequence, and the reactor was closed.

[0221] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;

[0222] Add vinylidene fluoride monomer into the reactor until the pressure inside the reactor reaches 7.5 MPa;

[0223] The temperature in the kettle was raised to 85°C to start the reaction. Vinylidene fluoride monomer was continuously introduced during the reaction to maintain the reaction pressure in the kettle constant.

[0224] When the amount of vinylidene fluoride monomer introduced reaches 80% of the total mass of the vinylidene fluoride monomer, 30.6 g of a 5% concentration potassium persulfate solution and 19.2 g of a 5% concentration sodium thiosulfate are added, and the reaction pressure is maintained while introducing a mixed gas of vinylidene fluoride monomer and butadiene into the reactor. The molar ratio of vinylidene fluoride monomer to butadiene monomer is 2:3.

[0225] When all 3783.7 g of vinylidene fluoride monomer is added and the amount of butadiene monomer added accounts for 50% of the total butadiene, the remaining 28.8 g of 5% sodium thiosulfate is added, and the remaining 931 g of butadiene monomer and 354.7 g of acrylic acid monomer are introduced into the reactor while maintaining the reaction pressure;

[0226] When the reaction is completed, the pressure in the autoclave drops to 0.2 MPa, and the unreacted butadiene monomer is recovered for reaction; the product is condensed, washed, separated, dried, and crushed to obtain a vinylidene fluoride-butadiene-acrylic acid copolymer binder.

[0227] 2) Preparation of insulation slurry

[0228] Add 13000g of N-methylpyrrolidone into a 35L stirred tank;

[0229] 700 g of the vinylidene fluoride-butadiene-acrylic acid copolymer powder prepared above was added to N-methylpyrrolidone, and the stirring speed was set to 1000 rpm for 60 minutes. After the stirring was completed, a prefabricated glue solution was obtained;

[0230] 6195 g of boehmite powder was added to the prefabricated glue solution, and the stirring speed was set to 1200 rpm for 60 minutes. The cooling water circulation in the stirring tank was started, and the stirring was completed to obtain a boehmite slurry;

[0231] 105 g of black zirconium oxide powder was added to the boehmite slurry, and the stirring speed was set to 1200 rpm for 60 minutes. The cooling water circulation in the stirring tank was started, and vacuum was started. After the stirring was completed, an insulating slurry was obtained.

[0232] 3) Preparation of insulating coating

[0233] The above insulating slurry was coated on a 13 μm aluminum foil with a coating thickness of 15±1 μm. The slurry was dried to form an insulating coating. The insulating coating was obtained on the other side of the aluminum foil using the same method. The thickness of the insulating coating on both sides plus the aluminum foil was 43±2 μm.

[0234] The preparation methods of the insulating coatings of Examples 2 to 26 and Comparative Examples 1 to 4 are similar to the preparation method of Example 1, except that the parameters for preparing the binder and the ratio of black zirconium dioxide in the slurry are adjusted.

[0235] In Examples 2 to 7, the ratios of the monomers in the binder were adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2.

[0236] In Examples 8-11, the reaction conditions for the binder synthesis were adjusted to achieve different weight-average molecular weights. Other parameters remained the same as in Example 6. Specific parameters are shown in Tables 1 and 2. Specifically, the preparation method for the fluoropolymer with a weight-average molecular weight of 500,000 in Example 8 was essentially the same as in Example 6, except that the amount of 5% potassium persulfate solution added was adjusted from 71.4 g to 78.54 g.

[0237] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 800,000 in Example 9 is basically the same as the steps in Example 6, except that the reaction temperature is adjusted from 85°C to 80°C, and the amount of 5% potassium persulfate solution added is adjusted from 71.4g to 67.83g.

[0238] The preparation method of the fluorinated polymer with a weight average molecular weight of 900,000 in Example 10 is basically the same as the steps in Example 6, except that the reaction temperature is adjusted from 85°C to 80°C, and the amount of 5% potassium persulfate solution added is adjusted from 71.4g to 64.26g.

[0239] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 400,000 in Example 11 is basically the same as the steps in Example 6, except that the amount of 5% potassium persulfate solution added is adjusted from 71.4 g to 82.11 g.

[0240] In Examples 12 to 15, the mass fraction of the binder in the slurry was adjusted, and other parameters remained the same as in Example 6. Specific parameters are shown in Tables 1 and 2.

[0241] In Examples 16-19, the solid content of the slurry was adjusted, and other parameters remained the same as in Example 6. Specific parameters are shown in Tables 1 and 2.

[0242] In Example 20, butadiene in the binder synthesis monomer is replaced by propylene, and other parameters remain the same as in Example 6. Specific parameters are shown in Tables 1 and 2.

[0243] In Example 21, the binder is a vinylidene fluoride-butadiene-acrylic acid copolymer prepared by a conventional method. The synthesis method is as follows: 30 kg of deionized water (conductivity less than or equal to 2 μs / cm), 21 g of an alkali metal perfluorooctanoate salt, and 71.4 g of a 5% concentration potassium persulfate solution are sequentially added to a reactor, and the reactor is closed.

[0244] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;

[0245] Add vinylidene fluoride monomer, butadiene monomer, and 720 g of acrylic acid monomer into the reactor until the pressure in the reactor reaches 7.5 MPa, wherein the molar ratio of vinylidene fluoride monomer to butadiene monomer is 8:1;

[0246] The temperature in the kettle was raised to 85°C to start the reaction. During the reaction, vinylidene fluoride monomer and butadiene monomer were continuously introduced to maintain the reaction pressure in the kettle constant. The total mass of the introduced vinylidene fluoride monomer and butadiene monomer were 5120 g and 540 g, respectively.

[0247] When the reaction is completed, the pressure in the autoclave drops to 0.0-0.5 MPa, and the unreacted butadiene monomer is recovered; the reaction product is condensed, washed, separated, dried, and crushed to obtain a vinylidene fluoride-butadiene-acrylic acid copolymer binder.

[0248] In Examples 22-26, the mass content of black zirconium dioxide in the slurry was changed, and other parameters remained the same as in Example 6. The specific parameters are shown in Table 3.

[0249] In Comparative Example 1, a vinylidene fluoride polymer is used as a binder, which is HSV900 model produced by Arkema, France.

[0250] In Comparative Example 2, the binder is a vinylidene fluoride-butadiene copolymer, and its synthesis method is basically the same as that in Example 1, except that when the vinylidene fluoride monomer is 80% of the total mass of the vinylidene fluoride monomer, 30.6 g of a 5% concentration potassium persulfate solution and 19.2 g of a 5% concentration sodium thiosulfate are added, and the reaction pressure is maintained. A mixed gas of vinylidene fluoride monomer and butadiene is introduced into the reactor, wherein the mass of butadiene in the mixed gas is 2160 g, and the mass of the vinylidene fluoride monomer is 756.7 g.

[0251] In Comparative Example 3, the binder is a vinylidene fluoride-acrylic acid copolymer, and its synthesis method is basically the same as that in Example 1, except that when the vinylidene fluoride monomer is 80% of the total mass of the vinylidene fluoride monomer, 30.6 g of 5% concentration potassium persulfate solution and 19.2 g of 5% concentration sodium thiosulfate are added, 2880 g of acrylic acid is added to the reactor to maintain the reaction pressure, and 756.7 g of vinylidene fluoride monomer is continued to be introduced.

[0252] In Comparative Example 4, the binder is a vinylidene fluoride-butadiene-acrylic acid copolymer, and its synthesis method is the same as that of Example 1, except that the molar content of the synthetic monomers is adjusted. For details, see Tables 1 and 2.

[0253] The relevant parameters of the insulating coatings of the above-mentioned Examples 1 to 26 and Comparative Examples 1 to 4 are shown in Tables 1, 2 and 3 below.

[0254] 2. Test Method

[0255] The insulating coatings obtained in Examples 1 to 26 and Comparative Examples 1 to 4 were subjected to performance tests. The test methods are as follows:

[0256] 1. Weight average molecular weight test

[0257] A Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141) was used. A 3.0% polystyrene solution sample was used as a reference, and a matching chromatographic column was selected (oily: Styragel HT5DMF7.8×300mm+Styragel HT4). A 3.0% fluoropolymer solution was prepared using purified N-methylpyrrolidone (NMP) solvent. The prepared solution was allowed to stand for one day before use. During the test, tetrahydrofuran was first drawn into a syringe and rinsed several times. Then 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. After the reading stabilized, the data was acquired and the weight-average molecular weight was read.

[0258] 2. Glue viscosity test

[0259] Dissolve the fluoropolymer in N-methylpyrrolidone (NMP) solvent to prepare a glue solution with a solid content of 7%. Select a suitable rotor, fix the viscometer, place the glue solution under the viscometer, and the slurry just submerges the scale line of the rotor. Instrument model: Shanghai Fangrui NDJ-5S, rotor: 62# (500-2500mPa·s), 63# (2500-10000mPa·s), speed: 12 rpm, test temperature: 25℃, test time: 5min, wait for the display to stabilize and read the data.

[0260] 3. Slurry viscosity test

[0261] Use a rotating viscometer to measure the viscosity of the slurry. Select a suitable rotor, fix the viscometer rotor, and place the slurry under the viscometer rotor so that the slurry just covers the rotor scale line. Instrument model: Shanghai Fangrui NDJ-5S, rotor: 63# (2000-10000mPa·s), 64# (10000-50000mPa·s), speed: 12 rpm, test temperature: 25℃, test time: 5 minutes, wait for the display to stabilize and read the data.

[0262] 4. Slurry solid content test

[0263] Solids content test method: Prepare a glass Petri dish and record the weight m1. Place a portion of the prepared slurry into the dish and record the total weight m2. Heat the dish in a drying oven at 120°C for 1 hour. Weigh the dried dish and record the weight m3. Solids content = [(m3 - m1) / (m2 - m1)] × 100%.

[0264] 5. Slurry fluidity test

[0265] After the slurry has been allowed to stand for 6 and 12 hours, take an appropriate amount of the slurry with a spatula and observe whether it flows smoothly. If it flows smoothly, it is considered OK. If it does not flow well, the slurry will become jelly-like or clumpy, indicating gelation, and it is considered NG.

[0266] 6. Slurry filtration performance test

[0267] First, determine the filter mesh size: 200 mesh. Cut the filter mesh into 25cm x 25cm pieces with scissors. Find a clean 500ml beaker and make sure it is clean. Fold the 200 mesh filter mesh into a triangle. Pour 500ml of slurry into the filter mesh over the top of the filter mesh, pouring all at once. Start recording the time when the slurry begins to flow from the tip of the filter mesh into the beaker. Record the time it takes to filter 300ml.

[0268] 7. Adhesion test

[0269] With reference to GB-T2790-1995 national standard "Test method for 180° peel strength of adhesive", the adhesion test process of the embodiments and comparative examples of the present application is as follows: Use a blade to cut a sample with a width of 30mm and a length of 100-160mm, and stick a special double-sided tape on the steel plate. The tape is 20mm wide and 90-150mm long. Stick the insulating coating surface of the electrode sample cut earlier on the double-sided tape, and then roll it three times in the same direction with a 2kg roller. Fix a paper tape with a width equal to the electrode and a length of 250mm on the electrode collector and fix it with wrinkle glue. Turn on the power of the Sansi tensile testing machine (sensitivity is 1N), the indicator light is on, adjust the limit block to the appropriate position, and fix the end of the steel plate without the electrode with the lower clamp. Fold the paper tape upwards and fix it with the upper clamp, and use the "up" and "down" buttons on the manual controller attached to the tensile testing machine to adjust the position of the upper clamp. The test is then performed and the value is read at a tensile speed of 50 mm / min. The force at which the electrode is under force equilibrium is divided by the width of the tape as the bonding force of the insulating coating per unit length, which represents the bonding strength between the insulating coating and the current collector.

[0270] 8. Laser cutting test

[0271] A Dazzle laser die-cutting machine was used, with the laser output power set to 80% of the maximum output power and the laser frequency set to 1000KHz. The maximum cutting speed and cutting quality when cutting the pole pieces coated with insulating coatings in different embodiments were compared. If the CCD camera on the die-cutting machine can recognize it, it is judged as Y. If the CCD camera on the die-cutting machine cannot recognize it, it is judged as N. After laser cutting, the cross-sectional morphology after cutting is observed under an optical microscope. If there are obvious metal burrs on the cross-section after cutting, it is judged as failed; if there are no obvious metal burrs on the cross-section after cutting, it is judged as passed. Samples were taken from one hundred batches of cut products, and the pass rate of one hundred batches was calculated.

[0272] Table 1 Parameters and test results of Examples 1 to 21 and Comparative Examples 1 to 4

[0273]

[0274]

[0275] Table 2 Parameters and test results of Examples 1 to 21 and Comparative Examples 1 to 4

[0276]

[0277]

[0278] Table 3 Insulation coating cutting quality test

[0279]

[0280] Figure 8 is a microscopic image of the pole piece coated with an insulating coating after laser cutting in Example 26, wherein Figure 8A is a plan view of the pole piece cut, and Figure 8B is a cross-sectional view of the pole piece cut. Figure 9 is a microscopic image of the pole piece after laser cutting in Example 6, wherein Figure 9A is a plan view of the pole piece cut, and Figure 9B is a cross-sectional view of the pole piece cut. A comparison of Figures 8 and 9 shows that the pole piece with black zirconium dioxide added to the insulating coating has significantly reduced burr quantity and burr length after laser cutting, effectively improving the laser cutting quality of the pole piece.

[0281] According to the results of Table 1, the binders in Examples 1-21 are all fluoropolymers, comprising structural units derived from vinylidene fluoride, structural units derived from olefins (butadiene or propylene), and structural units derived from acrylic acid. The molar content of the structural units derived from vinylidene fluoride in the polymer is 60% to 80%, based on the total molar number of the structural units in the fluoropolymer. Good results have been achieved using the above-mentioned fluoropolymers as binders. Compared to the traditional PVDF binder in Comparative Example 1 and the fluoropolymer with a mass content of 90% derived from the vinylidene fluoride structural unit in Comparative Example 4, the fluoropolymers provided herein improve the slurry in terms of filterability and fluidity after standing for 6 hours. Compared to the vinylidene fluoride-butadiene copolymer and the vinylidene fluoride-acrylic acid copolymer in Comparative Examples 2 and 3, the fluoropolymers disclosed in the present application can comprehensively improve the fluidity, filterability, and bonding properties of the slurry, taking into account the processing properties and performance of the slurry.

[0282] From the comparison of Examples 1-3, 5-7 and Example 4, it can be seen that the molar content of the structural units derived from acrylic acid in the fluoropolymer is 5% to 20%. Based on the total molar number of all structural units in the fluoropolymer, the fluoropolymer also improves the fluidity of the slurry after standing for 12 hours, further broadening the process window of the slurry.

[0283] From the comparison of Examples 2-7 with Example 1, it can be seen that the molar content of the structural units derived from olefin monomers in the fluoropolymer is 5% to 30%, based on the total molar number of all structural units in the fluoropolymer. The fluoropolymer enables the slurry to improve the processing performance while taking into account the adhesion.

[0284] From the comparison of Examples 8-11, it can be seen that when the weight average molecular weight of the fluoropolymer is 500,000-800,000, the fluoropolymer can comprehensively improve the fluidity, filterability and bonding properties of the slurry, while taking into account the processing performance and usage performance of the slurry.

[0285] As shown in Examples 1-20, the viscosity of a 7% by weight slurry containing a fluoropolymer dissolved in N-methylpyrrolidone, prepared from the fluoropolymer, ranges from 2500 to 5000 mPa·s. This eliminates the need for additional dispersants or thickeners to improve processing performance in insulating coating slurries prepared from the fluoropolymer, thereby increasing production efficiency and optimizing the production process.

[0286] From the comparison between Example 6 and Example 21, it can be seen that the fluorine-containing polymer prepared by the method disclosed in the present application can more effectively improve the filterability and fluidity of the slurry and improve the processing performance of the slurry than the fluorine-containing binder synthesized by the traditional method.

[0287] From the comparison between Examples 6, 22-25 and Example 26, it can be seen that the addition of black zirconium oxide to the insulating coating is beneficial to reducing the burrs generated on the edge of the pole piece during laser cutting, improving the quality of the pole piece laser cutting, and improving the quality of the pole piece.

[0288] From the comparison between Examples 6, 23-24 and Examples 22 and 25, it can be seen that when the mass content of black zirconium oxide in the insulating coating is 0.2%-3%, the speed of laser cutting is improved, which helps to further improve production efficiency and increase production capacity; and the color difference between the insulating coating and the positive electrode active material layer enables the laser cutting equipment to accurately locate and identify, thereby improving processing accuracy.

[0289] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A fluorine-containing polymer, characterized in that It comprises a structural unit derived from a monomer represented by formula I, a structural unit derived from an olefin monomer, and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of the structural units in the fluorinated polymer. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen or substituted or unsubstituted C 1-5 alkyl.

2. The fluorinated polymer according to claim 1, wherein R1 is fluorine, R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl, and R5 and R6 are each independently selected from hydrogen or methyl.

3. The fluorinated polymer according to claim 1 or 2, characterized in that The molar content of the structural unit derived from the monomer represented by formula II is 5% to 25%, based on the total molar number of all structural units in the fluorine-containing polymer.

4. The fluorinated polymer according to any one of claims 1 to 3, characterized in that The molar content of the structural unit derived from the olefin monomer is 5% to 30%, based on the total molar number of all structural units in the fluorine-containing polymer.

5. The fluorine-containing polymer according to any one of claims 1 to 4, characterized in that The weight average molecular weight of the fluorine-containing polymer is 500,000-800,000.

6. The fluorinated polymer according to any one of claims 1 to 5, characterized in that The viscosity of the adhesive prepared by dissolving the fluorine-containing polymer in N-methylpyrrolidone is 1000-3000 mPa·s, and the mass content of the fluorine-containing polymer in the adhesive is 7%, based on the total mass of the adhesive.

7. The fluorine-containing polymer according to any one of claims 1 to 6, characterized in that The monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

8. The fluorinated polymer according to any one of claims 1 to 7, characterized in that The olefin monomer is selected from one or more of propylene, 2-butene, and butadiene.

9. The fluorine-containing polymer according to any one of claims 1 to 8, characterized in that The monomer represented by formula II is selected from one or both of acrylic acid and methacrylic acid.

10. A method for preparing a fluorine-containing polymer, characterized in that: The following steps are involved: A fluorine-containing polymer is prepared by polymerizing at least one monomer represented by formula I, at least one olefin monomer, and at least one monomer represented by formula II under polymerizable conditions, wherein the molar content of the monomer represented by formula I is 60% to 80%, based on the total molar number of the monomer represented by formula I, the olefin monomer, and the monomer represented by formula II. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 alkyl.

11. The preparation method according to claim 10, characterized in that: R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

12. The preparation method according to claim 10 or 11, characterized in that: The polymerization reaction comprises the following steps: First stage polymerization: providing a first initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure; Second stage polymerization: After a period of reaction, olefin monomer and monomer represented by formula II are fed into the reaction vessel for second stage polymerization; when the pressure in the reaction vessel drops to less than or equal to 0.5 MPa, the reaction is stopped, solid-liquid separation is performed, and the solid phase is retained.

13. The preparation method according to claim 12, characterized in that The initial reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 70° C. to 90° C.

14. The preparation method according to claim 12 or 13, characterized in that: The second stage polymerization comprises the following steps: When the mass of the monomer represented by formula I fed in is 70% to 85% of the total mass of the monomer represented by formula I supplied during the polymerization reaction, a mixed gas of the monomer represented by formula I and an olefin monomer is fed into the reaction vessel, and the initial reaction pressure is maintained to continue the reaction; After all the monomers represented by formula I are fed into the reaction container, a mixture of olefin monomers and monomers represented by formula II is fed into the reaction container.

15. The preparation method according to any one of claims 10 to 14, characterized in that The ratio of the total moles of the olefin monomers supplied during the polymerization reaction to the total moles of the monomers represented by formula I is 1:16-1:

2.

16. The preparation method according to any one of claims 10 to 15, characterized in that During the polymerization reaction, the ratio of the total molar number of the monomers represented by formula II supplied to the total molar number of the monomers represented by formula I is 1:16-1:

3.

17. The preparation method according to claim 14, characterized in that In the mixed gas, the molar ratio of the olefin monomer to the monomer represented by formula I is 1:1-2:

1.

18. The preparation method according to claim 14 or 17, characterized in that: In the mixture, the molar ratio of the olefin monomer to the monomer represented by formula II is 3:1-4:

1.

19. The preparation method according to claim 14 or 18, characterized in that: The second stage polymerization further comprises the following steps: Before feeding the mixed gas of the monomer represented by Formula I and the olefin monomer into the reaction container, the first initiator and the second initiator are added into the reaction container.

20. The preparation method according to claim 14 or 19, characterized in that: The second stage polymerization further comprises the following steps: Before feeding the mixture of olefin monomer and monomer represented by formula II into the reaction container, a second initiator is added into the reaction container.

21. The preparation method according to claim 19, characterized in that The first initiator is persulfate.

22. The preparation method according to claim 21, characterized in that The persulfate is selected from one or more of potassium persulfate and ammonium persulfate.

23. The preparation method according to claim 19 or 20, characterized in that The second initiator is thiosulfate.

24. The preparation method according to claim 23, characterized in that The thiosulfate is selected from sodium thiosulfate.

25. Use of the fluorine-containing polymer according to any one of claims 1 to 9 in a secondary battery.

26. An insulating coating comprising a binder and an inorganic insulating material, characterized in that: The binder is the fluorine-containing polymer according to any one of claims 1 to 9.

27. The insulating coating according to claim 26, characterized in that The binder has a mass content of 7.0% to 13.0%, based on the total mass of the insulating coating.

28. The insulating coating according to claim 26 or 27, characterized in that The inorganic insulating material comprises colored oxides, and the colored oxides are selected from one or more of black zirconium dioxide, yellow zirconium dioxide, red zirconium dioxide, and green zirconium dioxide.

29. The insulating coating according to any one of claims 26 to 28, characterized in that The mass content of the colored oxide is 0.2%-3%, based on the total mass of the insulating coating.

30. A method for preparing an insulating coating, characterized in that: The following steps are involved: Dispersing a binder in a solvent to prepare a glue solution, wherein the binder is a fluorine-containing polymer according to any one of claims 1 to 9; Mixing the inorganic insulating material with the glue and stirring to prepare a slurry, wherein the solid content of the slurry is 30%-40%; The slurry is coated on a current collector to prepare an insulating coating.

31. The method for preparing an insulating coating according to claim 30, wherein: When the solid content of the slurry is 30%-40%, the viscosity of the slurry is 2500-4000 mPa·s.

32. The method for preparing an insulating coating according to claim 30 or 31, characterized in that: The mixing of the inorganic insulating material and the glue comprises the following steps: The inorganic insulating material except the colored oxide is mixed with the glue, stirred, and then the colored oxide is added and stirred again to prepare the slurry.

33. A secondary battery, characterized in that: It comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, and the positive electrode sheet and / or the negative electrode sheet comprises the insulating coating according to any one of claims 26 to 29.

34. The secondary battery according to claim 33, characterized in that The secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.

35. A battery module, characterized in that: Includes the secondary battery according to claim 33 or 34.

36. A battery pack, characterized in that: Includes at least one of the secondary battery according to claim 33 or claim 34, and the battery module according to claim 35.

37. An electrical device, characterized in that: It includes at least one selected from the secondary battery of claim 33 or claim 34, the battery module of claim 35, and the battery pack of claim 36.

Citation Information

Cited By

  • Monomer cell and battery device

    CN122315291A

  • Monobloc cell and battery device

    CN122315291B