Method for preparing targeted catalytic membrane based on surface molecular imprinting nanometer material and application of targeted catalytic membrane
By preparing targeted catalytic membranes based on surface molecularly imprinted nanomaterials, combined with advanced oxidation technology, the problem of low removal efficiency of low-concentration sulfonamide pollutants in water is solved, rapid identification and efficient degradation are achieved, and the recovery and recycling performance of the catalyst are improved. .
Patent Information
- Application Number
- CN202410757538.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
When existing technology removes low-concentration sulfonamide pollutants from water, the nanoparticle contact efficiency is low, the catalytic activity and mass transfer efficiency are reduced, and the catalyst separation, recovery and recycling are difficult, resulting in low removal efficiency.
Targeted catalytic membranes are prepared based on surface molecularly imprinted nanomaterials. By mixing sulfamethoxazole with functional monomers and catalyst base nanoparticles, they undergo water bath treatment and polymerization to form a casting liquid and prepare a membrane with specific recognition capabilities. Targeted catalytic membrane, combined with advanced oxidation technology, degrades pollutants.
It achieves rapid identification and efficient degradation of sulfonamide pollutants, increases the contact rate between free radicals and pollutants, reduces the difficulty of catalyst agglomeration and recovery, improves recycling performance and oxidation efficiency, and is suitable for low- to medium- to low-temperature applications in various water bodies. Removal of concentrated pollutants.
Smart Images

Figure CN118767916A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution control, and specifically relates to a method for preparing a targeted catalytic membrane based on surface molecular imprinting nanomaterials and its application. Background Art
[0002] Sulfonamides are widely used as antibiotics and have a high detection rate in the environment, becoming a new pollutant. Although the concentration of sulfonamide antibiotics in water is low, they are difficult to remove by conventional methods due to their low adsorption coefficient and long retention time in water. Therefore, how to effectively remove sulfonamide pollutants in water has become one of the hot topics in water pollution treatment research.
[0003] Advanced oxidation technology (AOPs) degrades antibiotics and other organic pollutants by generating highly active free radicals. It has the characteristics of fast reaction rate and simple operation, and has received extensive attention in the field of antibiotic wastewater treatment. However, the efficient removal of low-concentration refractory pollutants by advanced oxidation technology has always been one of the key issues limiting its application. -4 s), low contact efficiency of nanoparticles, etc. For low concentration (microgram, nanogram / L) oxidation processes, low contact efficiency usually leads to high costs and low efficiency.
[0004] Catalysts prepared using molecularly imprinted nanoparticles usually have strong selectivity and targeting for low-concentration, difficult-to-degrade pollutants. The basic mechanism is to form an imprinted cavity with specific recognition ability for the target pollutant on the existing catalyst substrate through polymerization. Among them, surface molecular imprinting technology improves the selectivity of the material for the target molecule by preparing recognition sites that match the target pollutant on the catalyst surface, while further increasing the contact rate between free radicals and pollutants (Chemosphere.2020,240:124875).
[0005] However, molecular imprinted nanocatalysts also have problems in practical applications. First, although the traditional heterogeneous catalytic process can achieve good removal effects, its effective recovery has also become a difficulty in its application, just like traditional materials. This severely limits the economic efficiency of imprinted materials with higher preparation costs. Secondly, due to the layered structural characteristics of molecular imprinted nanoparticles, collisions, accumulation and other processes during actual applications will also cause damage and shelling of the imprinted layer, restricting its recycling performance. Finally, although molecular imprinted nanoparticles have targeted catalytic capabilities, the mass transfer process of free radicals has not improved, mainly manifested in the inability to more effectively contact the target substance within a limited mass transfer distance. Therefore, the selective removal of sulfonamide pollutants in deep advanced oxidation processes still faces huge challenges. Summary of the invention
[0006] In order to overcome the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method and application of preparing a targeted catalytic film based on surface molecular imprinted nanomaterials.
[0007] The present invention aims to solve the problems of low contact efficiency of existing nanoparticles, reduced catalytic activity and mass transfer efficiency caused by collision and accumulation during application, and low separation, recovery and recycling of nanocatalysts, and provides a targeted catalytic membrane that can specifically identify sulfonamide pollutants and quickly catalyze their degradation. The catalytic membrane has the advantages of accurate identification, fast pollutant degradation and a wide range of applications.
[0008] The purpose of the present invention is achieved by at least one of the following technical solutions:
[0009] According to the first invention, the present invention provides a method for preparing a targeted catalytic film based on surface molecular imprinted nanomaterials, the method comprising the following steps:
[0010] (1) dissolving sulfamethoxazole in ethanol, adding functional monomer and divinylbenzene, mixing evenly, standing, then adding catalyst base nanoparticles and NN azobisisobutyronitrile and introducing nitrogen to obtain a mixed solution; heating the mixed solution in a water bath to obtain a product after water bath treatment;
[0011] (2) filtering the product after the water bath treatment in step (1), separating the filtrate and the filter residue, then washing the filter residue with water or ethanol, and vacuum drying to obtain the surface molecularly imprinted nanomaterial;
[0012] (3) The nanoparticles obtained in step (2) are dispersed in an N,N-dimethylformamide (DMF) solution, polyvinylidene fluoride (PVDF) particles are added, and a casting liquid is formed under water bath conditions. The casting liquid is placed in a water bath to degas; a certain amount of the casting liquid is taken to form a film with uniform thickness to obtain a targeted catalytic film.
[0013] Furthermore, the catalyst substrate includes one or more of activated carbon, Fe3O4, hydrothermal carbon, and Fe-MOFs materials with a particle size less than 300nm; nano Fe3O4 is preferred.
[0014] Furthermore, the functional monomer in step (1) includes one or more of acrylamide, acrylic acid, 4-vinylpyridine, and methyl acrylate; preferably acrylamide.
[0015] Furthermore, the sulfonamide pollutant in step (1) is one or more of sulfonamide, sulfamethoxazole, sulfadimethoxine, sulfadiazine, sulfathiazole, sulfachloropyrazine and sulfadimethoxine; the molar ratio of the sulfonamide pollutant, divinylbenzene, functional monomer, catalyst substrate, ethanol, and NN azobisisobutyronitrile is 1:2-3:4-4.5:2-2.5:280-310:0.35-0.45, and the thickness of the imprinted layer of the prepared molecular imprinted catalyst is less than 300nm under this ratio.
[0016] Preferably, the standing time in step (1) is 12 hours; the temperature of the water bath heating treatment is 65°C, and the water bath heating treatment conditions are sealed heating prepolymerization at 50°C for 1 hour, and sealed heating polymerization at 65°C for 10 hours.
[0017] Preferably, during the water bath heating treatment in step (1), the mixture is shaken once every 0.5 h.
[0018] Furthermore, the vacuum drying temperature in step (2) is 60-80° C., and the drying time is 2-6 hours.
[0019] Preferably, the separation of the filtrate and the filter residue in step (2) can be carried out by magnetic separation or centrifugal separation (magnetic separation is used when Fe3O4 is used as the catalyst substrate), and then the precipitate (solid) is collected.
[0020] Preferably, the number of times of washing with water or ethanol in step (2) is 3-6 times. Washing with water and ethanol can remove the sulfonamide contaminant template molecules in the imprinting system.
[0021] Furthermore, the molar ratio of the amount of DMF added in step (3): the amount of PVDF particles (calculated based on a molecular weight of 64) added is 0.078-0.260: 0.008-0.034; the solution is stirred continuously before coating at a rate of 60-120 rpm (manual stirring is used when Fe3O4 is used as the catalyst substrate), and ultrasonic dispersion is prohibited; the mass ratio of the surface molecular imprinted nanoparticles loaded on the polyvinylidene fluoride is 4%-400%. The ratio of the film thickness to the molecular imprinted catalyst particle diameter is not less than 200:1.
[0022] Furthermore, in step (3), the water bath temperature is 65-75°C; the degassing time is 20min-60min; the degassing temperature is 40-50°C, and the membrane standing time is 5min-20mim.
[0023] Preferably, the degassing temperature in step (3) is 45° C., the degassing is performed for 30 min, and the film is allowed to stand for 10 min.
[0024] Preferably, the above preparation method can be specifically as follows:
[0025] (1) In a 20 mL centrifuge tube, 0.23 g of sulfamethoxazole was dissolved in 16 mL of ethanol, and 0.28 g of functional monomer acrylamide and 0.3 mL of divinylbenzene were added, mixed evenly, and allowed to stand for 6-18 hours. Then, 0.5 g of catalyst substrate nano Fe3O4 particles and 60 mg of NN azobisisobutyronitrile were added, and nitrogen was introduced, and the lid was closed. The resulting mixed solution was heated in a sealed water bath at a temperature of 50 ° C for prepolymerization for 1 hour, and heated in a sealed water bath at a temperature of 65 ° C for polymerization for 10 hours, and shaken once every 30 minutes to obtain the product after water bath treatment;
[0026] (2) filtering the product after the water bath treatment in step (1), separating the filtrate and the filter residue, and drying the obtained filter residue in an electric heated forced air drying oven at a temperature of 80° C. for 2 h to obtain surface molecularly imprinted nanoparticles, which were placed in a 10 mL centrifuge tube for later use;
[0027] (3) Take 0.5g of the nanoparticles obtained in step (2) and disperse them in 10mL of N,N-dimethylformamide solution (DMF) in a 100mL beaker, add 1.25g of polyvinylidene fluoride particles (PVDF), stir manually for 2h in a 70℃ water bath to form a viscous and uniform casting solution, and place the casting solution in a 45℃ water bath for degassing for 30min. Take a certain amount of casting solution and apply it to a 20*40cm glass plate with a 400μm scraper (or coater) to form a film of uniform thickness. After the film is allowed to stand for 10min, it is immersed in mild deionized water. After the film is completely formed, it is repeatedly rinsed with ethanol and stored in a water and ethanol solution with a volume ratio of 1:1 for use. The obtained material is recorded as a targeted catalytic membrane, i.e., MIP membrane.
[0028] According to a second aspect, the present invention also provides a targeted catalytic membrane, namely, a MIP membrane, prepared by the above-mentioned preparation method.
[0029] According to a third aspect, the present invention also provides use of the targeted catalytic membrane in removing sulfonamide pollutants from wastewater.
[0030] Furthermore, the application of the targeted catalytic membrane in removing sulfonamide pollutants in wastewater comprises the following steps:
[0031] Take 100mL of 0.5mg / L sulfamethoxazole concentrated solution in a beaker and add 0.119mL of 50mmol / L persulfate solution potassium persulfate at a molar ratio of 1:30, and mix the solution. Cut the prepared membrane into a 25mm circle and put it into a replaceable membrane filter. Use a 30mL syringe to draw an appropriate amount of solution, connect the replaceable membrane filter and the syringe, and install it on the injection pump, set the flow rate to 50μL / min, and conduct a catalytic degradation experiment of the membrane to obtain treated water with sulfamethoxazole removed.
[0032] Furthermore, the concentration of the sulfonamide pollutants is less than 2.5 mg / L; the persulfate is one or more of potassium persulfate, sodium persulfate and potassium persulfate; the molar ratio of the persulfate to the sulfonamide pollutants in the wastewater is 10-100:1; the solution membrane flux is 0.05-0.41 L / m 2 ·h.
[0033] Preferably, the molar ratio of persulfate to sulfonamide pollutants in the wastewater is 30:1.
[0034] The present invention combines catalytic materials, membrane separation technology and advanced oxidation technology, which can complement each other and give full play to the advantages of the three, solving the problems of easy agglomeration of nanocatalysts, difficulty in separation and recovery of nanocatalysts and low recycling rate, while improving catalytic efficiency. The present invention uses the surface molecular imprinting layer and active center of the targeted catalytic membrane to achieve rapid activation of oxidants and targeted removal of pollutants, and realizes the fixation and recovery of molecular imprinted nanoparticles and rapid mass transfer of free radicals through the confined environment of the polymer membrane pores, thereby achieving efficient degradation of pollutants. Among them, surface molecular imprinting technology can improve the selectivity of materials for target pollutant molecules, and at the same time increase the contact rate between free radicals and pollutants; advanced oxidation technology AOPs degrades antibiotics and other organic pollutants by producing highly active free radicals, and has the characteristics of fast reaction rate and simple operation. Multiphase AOPs based on nanomaterials can promote electron transfer and the generation of reactive oxygen, and show excellent antibiotic pollutant removal efficiency; separation membranes have controllable pore size and high porosity, and the tortuous membrane pore channels can provide abundant loading sites for nanocatalysts, realizing physical separation and chemical oxidation simultaneously; and the oxidation reaction triggered during membrane filtration also gives AOPs the advantage of continuous operation.
[0035] Due to the strong anti-interference ability of molecularly imprinted nanoparticles, the removal efficiency of the material for the difficult-to-degrade sulfonamide pollutants in complex organic wastewater is significantly enhanced, and it is suitable for the rapid identification and targeted removal of low-concentration sulfonamide pollutants in various water bodies. This method has a short catalytic reaction time, accurate identification, no need to adjust the pH of the wastewater, low oxidant usage, and high degradation efficiency. The material has low operating costs, a wide range of applications, good economic benefits and broad application prospects.
[0036] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0037] (1) The preparation method provided by the present invention combines molecular imprinting technology, membrane technology and advanced oxidation technology to develop a targeted catalytic membrane, which achieves efficient adsorption of low-concentration organic pollutants and low-energy oxidative degradation, while enhancing the free radical mass transfer efficiency and improving the oxidation efficiency. Compared with traditional molecular imprinting materials under the same conditions, it can achieve higher oxidation efficiency and circulation capacity. Using N,N-dimethylformamide as a solvent and polyvinylidene fluoride as a membrane-forming material, the catalytic material is directly fixed in the membrane, which is easy to separate and recover.
[0038] (2) The catalytic material provided by the present invention for targeted removal of sulfonamide pollutants in wastewater by the catalytic membrane prepared based on surface molecular imprinting nanomaterials is less likely to agglomerate than traditional nanocatalysts, is better separated and recovered, can be recycled, has significantly enhanced water stability, and has stable catalytic degradation ability within the pH range.
[0039] (3) The catalytic material provided by the present invention is a catalytic membrane prepared based on surface molecular imprinting nanomaterials for targeted removal of sulfonamide pollutants in wastewater. The material has a strong selective recognition ability for sulfonamide pollutants and a high catalytic efficiency;
[0040] (4) The catalytic material provided by the present invention for targeted removal of sulfonamide pollutants from wastewater by the catalytic membrane prepared based on surface molecular imprinting nanomaterials has a wide range of applications and has certain practical application prospects;
[0041] (5) The catalytic material provided by the present invention for targeted removal of sulfonamide pollutants from wastewater based on the catalytic membrane prepared by surface molecular imprinting nanomaterials has a short reaction time, accurate identification, and no need to adjust the pH of the wastewater during the catalytic degradation of sulfonamide pollutants, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a comparison chart of the adsorption effects of PVDF membrane and MIP membrane.
[0043] Figure 2 This is a comparison chart of the catalytic effects of PVDF membrane and MIP membrane.
[0044] Figure 3 This is a comparison chart of the catalytic effects of MIP membrane and Fe3O4 membrane.
[0045] Figure 4 These are actual photos of the PVDF membrane, MIP membrane and Fe3O4 membrane obtained in Example 3. DETAILED DESCRIPTION
[0046] The specific implementation of the present invention is further described below in conjunction with examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0047] The present invention mainly uses sulfonamide, sulfamethoxazole and the like in organic wastewater as typical pollutants. The specific implementation of the present invention is further described below by way of examples, but the embodiments of the present invention are not limited thereto.
[0048] Example 1
[0049] (1) In a 20 mL centrifuge tube, 0.23 g of sulfamethoxazole was dissolved in 16 mL of ethanol, and 0.28 g of functional monomer acrylamide and 0.3 mL of divinylbenzene were added, mixed evenly, and allowed to stand for 6-18 hours. Then, 0.5 g of catalyst substrate nano Fe3O4 particles and 60 mg of NN azobisisobutyronitrile were added, and nitrogen was introduced, and the lid was closed. The resulting mixed solution was heated in a sealed water bath at a temperature of 50°C for prepolymerization for 1 hour, and heated in a sealed water bath at a temperature of 65°C for polymerization for 10 hours, and shaken once every 30 minutes to obtain a product after water bath treatment.
[0050] (2) The product obtained after water bath treatment in step (1) is filtered by magnetic separation to separate the filtrate and the residue. A rubidium magnet is placed on the beaker containing the product after water bath treatment (standing for 5-10 minutes) to separate the filtrate and the residue, and the obtained residue is repeatedly washed with water or ethanol until the filtrate is clear, the filtrate is removed, and the obtained residue is dried in an electric heating forced air drying oven at a temperature of 80° C. for 2 hours to obtain surface molecularly imprinted nanoparticles, which are placed in a 10 mL centrifuge tube for later use.
[0051] (3) Take two groups of 100mL beakers, add 10mL DMF and 1.25g PVDF to one group, marked as PVDF membrane; add 10mL DMF, 1.25g PVDF and 0.5g nanoparticles obtained in step (2) to the other group, marked as MIP membrane, stir manually for 2h in a 70℃ water bath to form a viscous and uniform casting solution, and place the casting solution in a 45℃ water bath for degassing for 30min. Take a certain amount of casting solution and apply it to a 20*40cm glass plate with a 400μm scraper (or applicator) to form a film of uniform thickness. After the film is allowed to stand for 10min, it is immersed in mild deionized water. After the film is completely formed, it is repeatedly rinsed with ethanol and stored in a water and ethanol solution with a volume ratio of 1:1 for use.
[0052] (4) The prepared membrane was cut into a 25 mm circle and placed in a replaceable membrane filter. 20 mL of a 0.5 mg / L sulfamethoxazole solution was drawn into a 30 mL syringe, the replaceable membrane filter and the syringe were connected and installed on a syringe pump, the flow rate was set to 50 μL / min, and the membrane adsorption experiment was performed to obtain treated water with sulfamethoxazole removed.
[0053] (5) The obtained PVDF membrane and MIP membrane have smooth surface, uniform thickness, stable properties, and certain plasticity and toughness. The PVDF membrane is white with a yellowish tint, and the MIP membrane is black.
[0054] The parameters of the selective adsorption effect of sulfamethoxazole on the PVDF membrane and the MIP membrane prepared in Example 1 are as follows: Figure 1 As shown, the results show that the MIP membrane has an adsorption effect on sulfamethoxazole pollutants, and the effect is significant.
[0055] Example 2
[0056] (1) In a 20 mL centrifuge tube, 0.23 g of sulfamethoxazole was dissolved in 16 mL of ethanol, and 0.28 g of functional monomer acrylamide and 0.3 mL of divinylbenzene were added, mixed evenly, and allowed to stand for 6-18 hours. Then, 0.5 g of catalyst substrate nano Fe3O4 particles and 60 mg of NN azobisisobutyronitrile were added, and nitrogen was introduced, and the lid was closed. The resulting mixed solution was heated in a sealed water bath at a temperature of 50°C for prepolymerization for 1 hour, and heated in a sealed water bath at a temperature of 65°C for polymerization for 10 hours, and shaken once every 30 minutes to obtain a product after water bath treatment.
[0057] (2) The product obtained in step (1) after water bath treatment is filtered by magnetic separation to separate the filtrate and the filter residue. The obtained filter residue is repeatedly washed with water or ethanol by magnetic separation until the filtrate is clear, the filtrate is poured out, and the obtained filter residue is dried in an electric heating forced air drying oven at a temperature of 80° C. for 2 h to obtain surface molecularly imprinted nanoparticles, which are placed in a 10 mL centrifuge tube for later use.
[0058] (3) Take two groups of beakers, add 10 mL DMF and 1.25 g PVDF to the first group, marked as PVDF membrane; add 10 mL DMF, 1.25 g PVDF and 0.5 g nanoparticles obtained in step (2) to the second group, marked as MIP membrane, manually stir for 2 h in a 70 ° C water bath to form a viscous and uniform casting solution, and place the casting solution in a 45 ° C water bath for degassing for 30 min. Take a certain amount of casting solution and apply it on a 20*40 cm glass plate with a 400 μm scraper (or applicator) to form a film of uniform thickness. After the film is allowed to stand for 10 min, it is immersed in mild deionized water. After the film is completely formed, it is repeatedly rinsed with ethanol and stored in a water and ethanol solution with a volume ratio of 1:1 for use.
[0059] (4) Take 100 mL of 0.5 mg / L sulfamethoxazole concentrated solution in a beaker, add 0.119 mL of 50 mmol / L persulfate solution potassium persulfate, the molar ratio is 1:30, and mix the solution. Cut the prepared membrane into a 25 mm circle and put it into a replaceable membrane filter. Use a 30 mL syringe to draw an appropriate amount of solution, connect the replaceable membrane filter and the syringe, and install it on the injection pump, set the flow rate to 50 μL / min, and conduct membrane adsorption and catalytic experiments to obtain treated water with sulfamethoxazole removed.
[0060] (4) The obtained PVDF membrane and MIP membrane have smooth surface, uniform thickness, stable properties, and certain plasticity and toughness. The PVDF membrane is white with a yellowish tint, and the MIP membrane is black.
[0061] Comparison of catalytic effects of the PVDF membrane and MIP membrane prepared in Example 2 Figure 2 The results show that compared with pure PVDF membrane, MIP membrane has a catalytic effect, and a significant catalytic effect, and the removal rate of sulfamethoxazole is fast.
[0062] Example 3
[0063] (1) In a 20 mL centrifuge tube, 0.23 g of sulfamethoxazole was dissolved in 16 mL of ethanol, and 0.28 g of functional monomer acrylamide and 0.3 mL of divinylbenzene were added, mixed evenly, and allowed to stand for 6-18 hours. Then, 0.5 g of catalyst substrate nano Fe3O4 particles and 60 mg of NN azobisisobutyronitrile were added, and nitrogen was introduced, and the lid was closed. The resulting mixed solution was heated in a sealed water bath at a temperature of 50°C for prepolymerization for 1 hour, and heated in a sealed water bath at a temperature of 65°C for polymerization for 10 hours, and shaken once every 30 minutes to obtain a product after water bath treatment.
[0064] (2) The product obtained in step (1) after water bath treatment is filtered by magnetic separation to separate the filtrate and the filter residue. The obtained filter residue is repeatedly washed with water or ethanol by magnetic separation until the filtrate is clear, the filtrate is poured out, and the obtained filter residue is dried in an electric heating forced air drying oven at a temperature of 80° C. for 2 h to obtain surface molecularly imprinted nanoparticles, which are placed in a 10 mL centrifuge tube for later use.
[0065] (3) Take two groups of beakers, the first group contains 0.5g of the nanoparticles obtained in step (2), marked as MIP membrane; the second group adds 10mL DMF, 1.25g PVDF and 0.5g nano-Fe3O4, marked as Fe3O4 membrane, and stirs manually for 2h in a 70℃ water bath to form a viscous and uniform casting solution, and the casting solution is placed in a 45℃ water bath for degassing for 30min. Take a certain amount of casting solution and apply it to a 20*40cm glass plate with a 400μm scraper (or applicator) to form a film of uniform thickness. After the film is allowed to stand for 10min, it is immersed in mild deionized water. After the film is completely formed, it is repeatedly rinsed with ethanol and stored in a water and ethanol solution with a volume ratio of 1:1 for later use.
[0066] (4) Take 100 mL of 0.5 mg / L sulfamethoxazole concentrated solution in a beaker, add 0.119 mL of 50 mmol / L persulfate solution potassium persulfate, the molar ratio is 1:30, and mix the solution. Cut the prepared membrane into a 25 mm circle and put it into a replaceable membrane filter. Use a 30 mL syringe to draw an appropriate amount of solution, connect the replaceable membrane filter and the syringe, and install it on the injection pump, set the flow rate to 50 μL / min, and conduct membrane adsorption and catalytic experiments to obtain treated water with sulfamethoxazole removed.
[0067] (5) The obtained PVDF membrane, MIP membrane and Fe3O4 membrane have smooth surface, uniform thickness, stable properties, and certain plasticity and toughness. The MIP membrane and Fe3O4 membrane are all black (such as Figure 4 shown).
[0068] Comparison of the catalytic effects of the MIP membrane and Fe3O4 membrane prepared in Example 2 Figure 3 Nano-Fe3O4 itself has a certain catalytic effect, and the prepared MIP membrane still has a catalytic effect significantly higher than that of the Fe3O4 membrane, indicating that the MIP membrane has a significant catalytic effect and the removal rate of sulfamethoxazole is faster.
Claims
1. A method for preparing a targeted catalytic film based on surface molecular imprinted nanomaterials, characterized in that: The steps include: (1) dissolving sulfamethoxazole in ethanol, adding functional monomer and divinylbenzene, mixing evenly, standing, then adding catalyst substrate and NN azobisisobutyronitrile and introducing nitrogen to obtain a mixed solution; heating the mixed solution in a water bath to obtain a product after water bath treatment; (2) filtering the product after the water bath treatment in step (1), separating the filtrate and the filter residue, then washing the filter residue with water or ethanol, and vacuum drying at 60-80° C. for 4 h to obtain the surface molecularly imprinted nanoparticles; (3) The nanoparticles obtained in step (2) are dispersed in an N,N-dimethylformamide solution, polyvinylidene fluoride particles are added, and a casting liquid is formed under water bath conditions, and the casting liquid is degassed in a water bath; a certain amount of the casting liquid is taken to form a film with uniform thickness to obtain a targeted catalytic film.
2. The method according to claim 1, characterized in that: In step (1): The catalyst substrate includes one or more of activated carbon, Fe3O4, hydrothermal carbon, and Fe-MOFs materials with a particle size less than 300 nm; The functional monomers include one or more of acrylamide, acrylic acid, 4-vinylpyridine and methyl acrylate.
3. The method according to claim 1, characterized in that In step (1): The molar ratio of the sulfonamide pollutant, divinylbenzene, functional monomer, catalyst substrate, ethanol and NN azobisisobutyronitrile is 1:2-3:4-4.5:2-2.5:280-310:0.35-0.
45. Under this ratio, the thickness of the imprinted layer of the prepared molecular imprinted catalyst is less than 300nm.
4. The method according to claim 1, characterized in that: In step (1): The standing time is 6 to 18 hours; The water bath heating treatment temperature is 50-75°C; The water bath heating treatment time is 6 to 12 hours.
5. The method according to claim 1, characterized in that In step (3): The molar ratio of N,N-dimethylformamide to polyvinylidene fluoride particles is 0.078-0.260:0.008-0.034; the solution is stirred continuously before coating at a rate of 60-120 rpm; the mass ratio of surface molecular imprinting nanoparticles loaded to polyvinylidene fluoride is 4%-400%.
6. The method according to claim 1, characterized in that In step (3): The ratio of the membrane thickness to the molecular imprinting catalyst particle diameter is not less than 200:
1.
7. The method according to claim 1, characterized in that In step (3): The water bath temperature is 65-75°C; The degassing time is 20 to 60 minutes; The degassing temperature is 40-50°C; The film is left to stand for 5 to 20 minutes.
8. A targeted catalytic film prepared by the method according to any one of claims 1 to 7.
9. Use of the targeted catalytic membrane according to claim 8 in removing sulfonamide pollutants from wastewater, characterized in that: The steps include: In a beaker, add a 0.5 mg / L sulfamethoxazole concentrated solution to a 50 mmol / L persulfate solution, with the molar ratio of sulfamethoxazole to persulfate being 1:30, and mix the solution; The prepared membrane is cut into a circular shape and placed in a replaceable membrane filter; A suitable amount of solution was drawn with a syringe, and the replaceable membrane filter and the syringe were connected and installed on a syringe pump. The flow rate and volume were set, and a membrane catalytic degradation experiment was conducted to obtain treated water from which sulfamethoxazole was removed.
10. The use according to claim 9, characterized in that: The concentration of the sulfonamide pollutant is less than 2.5 mg / L; The persulfate is one or more of potassium hydrogen persulfate, sodium persulfate and potassium persulfate; The molar ratio of the persulfate to the sulfonamide pollutants in the wastewater is 10 to 100:1; The solution membrane flux is 0.05 to 0.41 L / m 2 ·h.
Citation Information
Cited By
Preparation of solar photo-thermal conversion material with strong near-infrared light absorption and application of solar photo-thermal conversion material in degradation of organic pollutants