Ce monatomic loaded defect-rich LDH nano-catalyst and preparation method thereof

By introducing Ce single atoms into CoFe-LDH and using specific solvents and reaction conditions, defect-rich LDH nanocatalysts are formed, which solves the problems of poor conductivity and limited active sites of LDH materials, and achieves efficient electrocatalytic performance and large Large-scale production.

CN119020803APending Publication Date: 2024-11-26SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411416910.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing LDH materials have poor conductivity and limited active sites due to their block structure, which limits their application in the field of electrocatalysis and makes it difficult to achieve large-scale industrial production.

Method used

By introducing Ce single atoms into CoFe-LDH, reflux reaction is carried out using a mixed solvent of ethylene glycol and water and urea to form a Ce single atom-laden defect-rich LDH nanocatalyst, improving its conductive properties and active sites.

Benefits of technology

A high yield of Ce single-atom-loaded defective LDH nanocatalysts is achieved, with ultra-thin 2D nanosheet structure and rich pore structure, which improves electron conductivity and catalytic performance, and is suitable for large-scale production and electrocatalytic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020803A_ABST
    Figure CN119020803A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano materials, and discloses a Ce monatomic loaded defect-rich LDH nano catalyst and a preparation method thereof. The preparation method comprises the following steps: by taking a mixed solvent of ethylene glycol and water as a reaction solvent, sequentially adding a soluble ferric salt, a soluble cobalt salt, a soluble cerium salt and urea, uniformly mixing, then carrying out reflux reaction at 85-95 DEG C, so that iron ions provided by the soluble ferric salt and cobalt ions provided by the soluble cobalt salt form CoFe-LDH under the action of urea, meanwhile, cerium ions provided by soluble cerium salt are uniformly doped into CoFe-LDH in the form of Ce single atoms, and the Ce single atom loaded defect-rich LDH nano-catalyst is obtained. The preparation method disclosed by the invention is low in reaction temperature, short in reaction time, simple and high in yield of the generated catalyst; the prepared catalyst has excellent electronic conductivity and excellent electro-catalytic performance, and is beneficial to popularization and large-scale production and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a Ce single atom-loaded defect-rich LDH nanocatalyst and a preparation method thereof. Background Art

[0002] In recent years, layered double hydroxides, also known as LDHs, have emerged as water splitting electrocatalysts due to their unique layered structures and unique electron distribution. LDHs have been studied as valuable electrochemical oxygen evolution electrocatalysts due to their low-cost metal elements and highly flexible and tunable composition.

[0003] However, the LDH materials prepared by the existing technology are mostly blocky with large particle size and thickness, which usually leads to poor electronic conductivity and transport, and limits the exposure of active sites, resulting in poor conductivity and limited active sites of LDH materials. Compared with precious metal catalysts, their activity is poor, and their application in the field of electrocatalysis is restricted.

[0004] In order to solve the above technical problems, those skilled in the art have proposed that LDH can be controlled and synthesized by coprecipitation, hydrothermal synthesis or ion exchange in a low-saturated or high-saturated alkaline medium to obtain small-sized crystals. However, the above methods are mainly limited to laboratories, and the products prepared are at the milligram level with low yield, making it difficult to achieve large-scale industrial production. Summary of the invention

[0005] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a Ce single atom-loaded defect-rich LDH nanocatalyst and a preparation method thereof.

[0006] The Ce single atom-loaded defect-rich LDH nanocatalyst and the preparation method thereof of the present invention are achieved by the following technical solutions:

[0007] The first object of the present invention is to provide a method for preparing a Ce single atom-loaded defect-rich LDH nanocatalyst.

[0008] It should be noted that the present invention takes into account that CoFe-LDH has good electrical conductivity, which is beneficial to improving the electrical conductivity of the overall catalyst, so CoFe-LDH is preferred as the matrix material, and in order to improve the electrical conductivity and active sites of the CoFe-LDH material, the present invention attempts to introduce Ce single atoms on the basis of CoFe-LDH, and Ce has good redox properties. 3+ / Ce 4+The characteristic electronic configuration of CoFe-LDH enables modification and doping of CoFe-LDH materials by doping with Ce, thereby adjusting the crystallinity and size of the CoFe-LDH layers, and further improving the electrical conductivity and active sites of the CoFe-LDH materials. The present invention specifically implements the doping and introduction of Ce single atoms into CoFe-LDH materials by the following steps:

[0009] Step 1: Using a mixed solvent of ethylene glycol and water as a reaction solvent, adding a soluble iron salt, a soluble cobalt salt and a soluble cerium salt and mixing them evenly, and then adding urea and mixing them evenly to obtain a mixed solution.

[0010] Step 2, subjecting the mixed solution to a reflux reaction at 85° C. to 95° C. to obtain the Ce single atom-loaded defect-rich LDH nanocatalyst.

[0011] It should be noted that the present invention is to uniformly disperse soluble iron salt, soluble cobalt salt and soluble cerium salt in a solvent so that the soluble cerium salt is fully in contact with the soluble iron salt and the soluble cobalt salt; after urea is used as a precipitation promoter to fully contact each metal ion, in the subsequent reflux reaction process, the iron ions provided by the soluble iron salt and the cobalt ions provided by the soluble cobalt salt form CoFe-LDH under the action of urea. And in the process of forming CoFe-LDH, the cerium ions provided by the soluble cerium salt are uniformly doped in CoFe-LDH, because the cerium ions provided by the soluble cerium salt are +3 valence, the iron ions in CoFe-LDH are also +3 valence, +3 valence iron has strong oxidizing property, +3 valence cerium has strong reducibility, and the binding ability of Ce-Fe bond is strong, which will form cation defects on CoFe-LDH, and Ce and defects are combined in the form of Ce single atoms and uniformly doped in CoFe-LDH, to obtain Ce single atom-loaded defect-rich LDH nanocatalyst.

[0012] It should be noted that the present invention uses a mixed solution of ethylene glycol and water as the reaction solvent, so that the reaction solvent used has good solubility for soluble cerium salts, soluble iron salts and soluble cobalt salts, thereby reducing or avoiding the agglomeration phenomenon in the LDH preparation process, thereby increasing the active surface area and utilization rate of the catalyst.

[0013] The present invention does not limit the specific type of the soluble cerium salt used, as long as it can provide cerium ions. In some feasible embodiments of the present invention, the soluble cerium salt used can be selected from one or more of cerium chloride, cerium nitrate and cerium sulfate.

[0014] The present invention does not limit the specific type of the soluble iron salt used, as long as it can provide iron ions. In some feasible embodiments of the present invention, the soluble iron salt used can be selected from one or more of ferric nitrate, ferric sulfate and ferric chloride.

[0015] The present invention does not limit the specific type of the soluble cobalt salt used, as long as it can provide cobalt ions. In some feasible embodiments of the present invention, the soluble cobalt salt used can be selected from one or more of cobalt nitrate, cobalt sulfate and cobalt chloride.

[0016] In some preferred embodiments of the present invention, the molar ratio of soluble cerium salt, soluble iron salt and soluble cobalt salt is 0.1-0.5:1:4, so as to ensure that the doped soluble cerium salt can be doped into CoFe-LDH to obtain a Ce single atom-loaded defect-rich LDH nanocatalyst with uniform component distribution.

[0017] In some preferred embodiments of the present invention, the ratio of the mixed solution of ethylene glycol and water to the soluble cerium salt is 50mL~55mL:0.1mmol~0.5mmol, so as to further ensure that the mixed solution of ethylene glycol and water can fully dissolve the soluble cerium salt, soluble iron salt and soluble cobalt salt.

[0018] In some more preferred embodiments of the present invention, in the mixed solution of ethylene glycol and water, the volume ratio of ethylene glycol to water is 2 to 3:1.

[0019] In some feasible embodiments of the present invention, ultrasonic coordinated stirring is used for dispersion, and the ultrasonic power is 120W and the ultrasonic time is 10min to 15min to ensure that the urea and the various metal ions can be stirred evenly.

[0020] It should be noted that, in order to ensure that the components in the mixed solution are fully contacted and reacted in the solvent environment, the present invention preferably performs a reflux reaction under stirring to obtain the Ce single atom-loaded defect-rich LDH nanocatalyst.

[0021] In some preferred embodiments of the present invention, the reflux reaction time is 4 h to 8 h, so as to further ensure that the Ce single atom-loaded defect-rich LDH nanocatalyst can be obtained through the reflux reaction.

[0022] It can be understood that, since the reflux reaction is carried out in a solvent environment, the target product obtained, i.e., Ce single atom-loaded defect-rich LDH nanocatalyst, is also present in the solvent environment. In order to facilitate the utilization of the target product, the reaction solution obtained by the reflux reaction needs to be post-processed, i.e., the reaction solution needs to be firstly subjected to solid-liquid separation to obtain a solid component, and then the solvent and other impurities remaining on the surface of the solid component are removed by washing, and then dried to remove the detergent used for washing, i.e., a pure Ce single atom-loaded defect-rich LDH nanocatalyst is obtained. Among them, in some more preferred embodiments of the present invention, for ease of operation, solid-liquid separation is performed by centrifugation, and after removing the supernatant, ethanol and deionized water are added to continue centrifugation, and the operation is repeated until the pH of the supernatant is 6.8 to 7.2. In some more preferred embodiments of the present invention, the drying temperature is 55°C to 65°C, and the drying time is 8h to 16h.

[0023] The second object of the present invention is to provide a Ce single atom-loaded defect-rich LDH nanocatalyst prepared by the above preparation method.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention uses an ethylene glycol-water system as a reaction solvent, which can effectively achieve the dispersion of soluble cerium salt, soluble iron salt and soluble cobalt salt, so that the soluble cerium salt is fully contacted with the soluble iron salt and the soluble cobalt salt in the reaction solvent. After adding urea and mixing, a reflux reaction is carried out at 85° C. to 95° C. After urea is used as a precipitation promoter and fully contacts each metal ion, in the subsequent reflux reaction process, the iron ions provided by the soluble iron salt and the cobalt ions provided by the soluble cobalt salt form CoFe-LDH under the action of urea. In the process of forming CoFe-LDH, the cerium ions provided by the soluble cerium salt are uniformly doped in CoFe-LDH. Since the cerium ions provided by the soluble cerium salt are +3 valent, the iron ions in CoFe-LDH are also +3 valent, +3 valent iron has strong oxidizing properties, +3 valent cerium has strong reducing properties, and the binding ability of the Ce-Fe bond is strong, which will form cationic defects on CoFe-LDH. Ce combines with the defects and is uniformly doped in CoFe-LDH in the form of Ce single atoms, thereby obtaining Ce single atom-loaded defect-rich LDH nanocatalyst.

[0026] The preparation method of the present invention is simple, the reaction temperature is low, the reaction time is short, and the yield of the Ce single atom-loaded defect-rich LDH nanocatalyst obtained by the preparation method of the present invention is high, and a 10-gram level LDH product can be prepared, which is conducive to promotion and large-scale production.

[0027] The Ce single atom-loaded defect-rich LDH nanocatalyst of the present invention has an ultrathin 2D nanosheet structure, and the ultrathin 2D nanosheet structure has a large number of pore structures, that is, a defect-rich structure. These defect-rich structures are not only conducive to electrolyte diffusion, but also provide more active sites and adsorption centers for the catalyst, so that the Ce single atom can be loaded on the LDH, accelerate the charge transfer in the water electrolysis reaction process, and make the catalyst have higher electronic conductivity, so that the Ce single atom-loaded defect-rich LDH nanocatalyst prepared by the present invention has excellent electrocatalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The XRD spectra of Example 2, Example 5 and Comparative Example 3 are shown.

[0029] Figure 2 For Ce 0.2 Low magnification TEM image of / CoFe-LDH at 200nm scale.

[0030] Figure 3 For Ce 0.2 Low-magnification TEM image of / CoFe-LDH at 50nm scale.

[0031] Figure 4 For Ce 0.2 High magnification TEM image of / CoFe-LDH at 10nm scale.

[0032] Figure 5 For Ce 0.2 High magnification TEM image of / CoFe-LDH at 2nm scale.

[0033] Figure 6 It is the Tafel slope diagram of Comparative Examples 1 to 4.

[0034] Figure 7 These are the OER performance test results of Example 2, Example 5 and Comparative Example 3. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below.

[0036] Example 1

[0037] This embodiment provides a Ce single atom-loaded defect-rich LDH nanocatalyst, and the preparation method thereof is as follows:

[0038] Step 1: prepare a mixed solution:

[0039] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0040] 2) 1 mmol of Fe(NO3)2·6H2O, 4 mmol of Co(NO3)2·6H2O and 0.1 mmol of CeCl3·6H2O were placed in the reaction solvent obtained above and mixed evenly, then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0041] Step 2, reflux reaction:

[0042] The mixed solution was stirred and refluxed in an oil bath at 90°C for 6 h, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, and the Ce single atom-loaded defect-rich LDH nanocatalyst was obtained, which was named Ce 0.1 / CoFe-LDH.

[0043] Example 2

[0044] This embodiment provides a Ce single atom-loaded defect-rich LDH nanocatalyst, and the preparation method thereof is as follows:

[0045] Step 1: prepare a mixed solution:

[0046] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0047] 2) 1 mmol of Fe(NO3)2·6H2O, 4 mmol of Co(NO3)2·6H2O and 0.2 mmol of CeCl3·6H2O were placed in the reaction solvent obtained above and mixed evenly, then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0048] Step 2, reflux reaction:

[0049] The mixed solution was stirred and refluxed in an oil bath at 90°C for 6 h, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, and the Ce single atom-loaded defect-rich LDH nanocatalyst was obtained, which was named Ce 0.2 / CoFe-LDH.

[0050] Example 3

[0051] This embodiment provides a Ce single atom-loaded defect-rich LDH nanocatalyst, and the preparation method thereof is as follows:

[0052] Step 1: prepare a mixed solution:

[0053] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0054] 2) 1 mmol of Fe(NO3)2·6H2O, 4 mmol of Co(NO3)2·6H2O and 0.3 mmol of CeCl3·6H2O were placed in the reaction solvent obtained above and mixed evenly, then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 to 15 minutes to obtain a uniformly dispersed mixed solution.

[0055] Step 2, reflux reaction:

[0056] The mixed solution was stirred and refluxed in an oil bath at 90°C for 6 h, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, and the Ce single atom-loaded defect-rich LDH nanocatalyst was obtained, which was named Ce 0.3 / CoFe-LDH.

[0057] Example 4

[0058] This embodiment provides a Ce single atom-loaded defect-rich LDH nanocatalyst, and the preparation method thereof is as follows:

[0059] Step 1: prepare a mixed solution:

[0060] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0061] 2) Add 1 mmol of Fe(NO3)2·6H2O, 4 mmol of Co(NO3)2·6H2O and 0.4 mmol of CeCl3·6H2O to the reaction solvent obtained above and mix well, then add 37.5 mmol of urea and stir, and ultrasonicate the mixed system for 10 to 15 minutes to obtain a uniformly dispersed mixed solution.

[0062] Step 2, reflux reaction:

[0063] The mixed solution was stirred and refluxed in an oil bath at 90°C for 6 h, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, and the Ce single atom-loaded defect-rich LDH nanocatalyst was obtained, which was named Ce 0.4 / CoFe-LDH.

[0064] Example 5

[0065] This embodiment provides a Ce single atom-loaded defect-rich LDH nanocatalyst, and the preparation method thereof is as follows:

[0066] Step 1: prepare a mixed solution:

[0067] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0068] 2) 1 mmol of Fe(NO3)2·6H2O, 4 mmol of Co(NO3)2·6H2O and 0.5 mmol of CeCl3·6H2O were placed in the reaction solvent obtained above and mixed evenly, then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0069] Step 2, reflux reaction:

[0070] The mixed solution was stirred and refluxed in an oil bath at 90°C for 6 h, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, and the Ce single atom-loaded defect-rich LDH nanocatalyst was obtained, which was named Ce 0.5 / CoFe-LDH.

[0071] In the above-mentioned Examples 1 to 5 of the present invention, the total amount of the three metal salts and urea fed is 3.8 g to 4.4 g, and the mass of the Ce single atom-loaded defect-rich LDH nanocatalyst prepared in Examples 1 to 5 is 750 mg to 850 mg, that is, the mass of the Ce single atom-loaded defect-rich LDH nanocatalyst prepared by the present invention is 17.05% to 19.73% of the total raw material feed mass.

[0072] Moreover, the present invention can obtain more than 10g level of Ce single atom-loaded defect-rich LDH nanocatalyst by increasing the feed amount of each of the above embodiments by 15 times. This shows that the preparation method of the present invention can be used to prepare LDH products at the ten-gram level, which is conducive to promotion and large-scale production.

[0073] Comparative Example 1

[0074] This comparative example provides a CoFe-LDH nanocatalyst, and its preparation method is as follows:

[0075] Step 1: prepare a mixed solution:

[0076] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0077] 2) 1 mmol of Fe(NO3)2·6H2O and 2 mmol of Co(NO3)2·6H2O were placed in the reaction solvent obtained above and mixed evenly, and then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0078] Step 2, reflux reaction:

[0079] The mixed solution was stirred and refluxed for 6 hours under an oil bath reaction condition of 90°C, and a solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, thereby obtaining a CoFe-LDH nanocatalyst, which was named Co2Fe-LDH.

[0080] Comparative Example 2

[0081] This comparative example provides a CoFe-LDH nanocatalyst, and its preparation method is as follows:

[0082] Step 1: prepare a mixed solution:

[0083] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0084] 2) 1 mmol of Fe(NO3)2·6H2O and 3 mmol of Co(NO3)2·6H2O were placed in the reaction solvent obtained above and mixed evenly, and then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0085] Step 2, reflux reaction:

[0086] The mixed solution was stirred and refluxed under oil bath reaction conditions at 90°C for 6 hours, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, thereby obtaining a CoFe-LDH nanocatalyst, which was named Co3Fe-LDH.

[0087] Comparative Example 3

[0088] This comparative example provides a CoFe-LDH nanocatalyst, and its preparation method is as follows:

[0089] Step 1: prepare a mixed solution:

[0090] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0091] 2) 1 mmol of Fe(NO3)2·6H2O and 4 mmol of Co(NO3)2·6H2O were placed in the reaction solvent obtained above and mixed evenly, and then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0092] Step 2, reflux reaction:

[0093] The mixed solution was stirred and refluxed for 6 hours under oil bath reaction conditions at 90°C, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, thereby obtaining a CoFe-LDH nanocatalyst, which was named Co4Fe-LDH.

[0094] Comparative Example 4

[0095] This comparative example provides a CoFe-LDH nanocatalyst, and its preparation method is as follows:

[0096] Step 1: prepare a mixed solution:

[0097] 1) Mix 37.5 mL of ethylene glycol and 15 mL of deionized water to obtain a reaction solvent.

[0098] 2) 1 mmol of Fe(NO3)2·6H2O and 5 mmol of Co(NO3)2·6H2O were placed in the reaction solvent obtained above and mixed evenly, and then 37.5 mmol of urea was added and stirred, and the mixed system was ultrasonicated for 10 min to 15 min to obtain a uniformly dispersed mixed solution.

[0099] Step 2, reflux reaction:

[0100] The mixed solution was stirred and refluxed under oil bath reaction conditions at 90°C for 6 hours, and the solid component was obtained by centrifugation. The solid component was repeatedly washed by centrifugation with ethanol and deionized water until the pH of the supernatant in the centrifuge tube was 7, thereby obtaining a CoFe-LDH nanocatalyst, which was named Co5Fe-LDH.

[0101] Experimental Section

[0102] (I) XRD test

[0103] The present invention uses Ce in Example 2 0.2 / CoFe-LDH, Ce of Example 5 0.5 / CoFe-LDH and Co4Fe-LDH of comparative example 3 were taken as examples, and XRD tests were performed on them respectively, and the test results are as follows Figure 1 shown.

[0104] Figure 1 The XRD spectra of Example 2, Example 5 and Comparative Example 3 are shown in Table 1. Figure 3 From the standard card CoFe-LDH PDF#50-0235, it can be seen that both Example 2 and Example 5 have the peak of CoFe-LDH, which indicates that the catalyst material prepared by the method of the present invention has good crystallinity.

[0105] By comparing Example 2, Example 5 and Comparative Example 3 with CeO2PDF#75-0120, it can be seen that when the Ce content is increased to the amount in Example 5, the diffraction peak of CeO2 gradually appears in the prepared material. This may be because when the added Ce content is small, Ce preferentially combines with cation defects to form Ce single atoms, and when the Ce content is too much, the excess Ce combines with O to form Ce oxide CeO2, which in turn causes the existence form of Ce to change. Therefore, the preferred molar ratio of the soluble cerium salt, the soluble iron salt and the soluble cobalt salt of the present invention is 0.1 to 0.5:1:4. More preferably, the molar ratio of the soluble cerium salt, the soluble iron salt and the soluble cobalt salt is 0.1 to 0.3:1:4.

[0106] (II) TEM test

[0107] The present invention uses Ce in Example 2 0.2 / CoFe-LDH was taken as an example, and TEM test was carried out on it, and the test results are as follows Figure 2-Figure 5 shown.

[0108] in, Figure 2 For Ce 0.2 / Low magnification TEM image of CoFe-LDH at 200nm scale, Figure 3 For Ce 0.2 / CoFe-LDH at 50nm scale, by Figure 2 and Figure 3 It can be seen that the Ce in Example 2 0.2 / CoFe-LDH has a unique porous nanosheet array network that provides a larger specific surface area, exposing more active sites.

[0109] Figure 4 For Ce 0.2 / CoFe-LDH at 10nm scale, it can be seen that Ce 0.2 / CoFe-LDH presents a nanosheet structure, and there are obvious defects on the nanosheet, which indicates that the Ce single atom-loaded defect-rich LDH nanocatalyst prepared by the present invention does have an ultra-thin 2D nanosheet structure, and the ultra-thin 2D nanosheet structure has a defect-rich structure.

[0110] Figure 5 For Ce 0.2 / CoFe-LDH at 2nm scale, it can be seen that Ce 0.2 There are obvious Ce single atoms in the defect structure of ultrathin 2D nanosheets of / CoFe-LDH, such as Figure 5 The position of the circle.

[0111] (III) OER performance test

[0112] In order to explore the effect of different ratios of Co and Fe on the performance of the catalyst, the present invention takes Co2Fe-LDH of Comparative Example 1, Co3Fe-LDH of Comparative Example 2, Co4Fe-LDH of Comparative Example 3 and Co5Fe-LDH of Comparative Example 4 as examples, and tests the Tafel slopes thereof respectively, and the test results are as follows: Figure 6 shown.

[0113] Figure 6 The Tafel slope diagrams of Comparative Examples 1 to 4 are shown in FIG. 1 . The lower the Tafel slope, the better the electrocatalytic performance. Figure 6 It can be seen that when the ratio of Co to Fe is 4 to 1, the Tafel slope of Co4Fe-LDH of comparative example 3 is the lowest and the electrocatalytic performance is the best. Therefore, the present invention introduces Ce on the basis of CoFe-LDH constructed with a ratio of Co to Fe of 4 to 1, so as to further improve the catalytic performance of CoFe-LDH through Ce.

[0114] In order to further explore the effect of different Ce contents on the catalytic performance improvement of CoFe-LDH, the present invention uses the Ce content of Example 2 as the 0.2 / CoFe-LDH, Ce of Example 5 0.5 Taking the Co4Fe-LDH of Example 3 and CoFe-LDH of Comparative Example 3 as examples, the OER performance tests were carried out respectively, and the test method was linear sweep voltammetry, and the specific test conditions were:

[0115] Carbon electrode was used as counter electrode, Ag / AgCl 1.0 M NaOH, and baseline conditions were used as reference electrode. A 1 × 1 cm nickel foam substrate coated with active materials was used as working electrode, and the loading of nanocatalyst was about 1.2 mg cm -2 In the water splitting evaluation, 1.0 M KOH was used as the electrolyte, and the nickel foam coated with the nanocatalyst was used as the electrode for the hydrogen evolution reaction and tested at 5 mV·s -1 The linear sweep voltammetry test was performed from 0V to -2V at a scan rate of Figure 7 shown.

[0116] Figure 7The OER performance test results of Example 2, Example 5 and Comparative Example 3 show that Ce 0.2 The / CoFe-LDH sample exhibits a relatively low overpotential value of 336 mV among the tested samples. This is much lower than the others, indicating that Ce 0.2 / CoFe-LDH has the best catalytic performance, which indicates that too much or too little Ce content cannot effectively improve the catalytic performance of CoFe-LDH. Therefore, the molar ratio of the soluble cerium salt, the soluble iron salt and the soluble cobalt salt is preferably 0.1-0.5:1:4 in the present invention, and more preferably 0.2:1:4.

[0117] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A method for preparing a Ce single atom-loaded defect-rich LDH nanocatalyst, characterized in that: The following steps are involved: Using a mixed solvent of ethylene glycol and water as a reaction solvent, adding a soluble iron salt, a soluble cobalt salt and a soluble cerium salt and mixing them evenly, and then adding urea and mixing them evenly to obtain a mixed solution; The mixed solution is subjected to a reflux reaction at 85° C. to 95° C., so that the iron ions provided by the soluble iron salt and the cobalt ions provided by the soluble cobalt salt form CoFe-LDH under the action of urea, and at the same time, the cerium ions provided by the soluble cerium salt are uniformly doped into CoFe-LDH in the form of Ce single atoms, thereby obtaining the Ce single atom-loaded defect-rich LDH nanocatalyst.

2. The preparation method according to claim 1, characterized in that The soluble cerium salt is one or more of cerium chloride, cerium nitrate and cerium sulfate.

3. The preparation method according to claim 1, characterized in that: The soluble iron salt is one or more of ferric nitrate, ferric sulfate and ferric chloride; The soluble cobalt salt is one or more of cobalt nitrate, cobalt sulfate and cobalt chloride.

4. The preparation method according to claim 1, characterized in that: The molar ratio of the soluble cerium salt, the soluble iron salt and the soluble cobalt salt is 0.1-0.5:1:

4.

5. The preparation method according to claim 1, characterized in that: The molar ratio of the urea to the soluble cobalt salt is 0.037-0.038:

1.

6. The preparation method according to claim 1, characterized in that: In the reaction solvent, the volume ratio of ethylene glycol to water is 2 to 3:

1.

7. The preparation method according to claim 1, characterized in that: The dosage ratio of the reaction solvent to the soluble cerium salt is 50 mL to 55 mL: 0.1 mmol to 5 mmol.

8. The preparation method according to claim 1, characterized in that: Ultrasonic coordinated stirring is used for dispersion, and the ultrasonic power is 120W, and the ultrasonic time is 10min to 15min.

9. The preparation method according to claim 1, characterized in that: The reflux reaction time is 4h to 8h.

10. A Ce single atom-loaded defect-rich LDH nanocatalyst prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Atomic-scale dispersed cerium-loaded photocatalyst, photocatalyst peculiar smell removal spray and preparation method and application of photocatalyst peculiar smell removal spray