Preparation method for improving compressibility of superfine W-Y2O3 powder large-size block by adding W powder
By adding tungsten powder to ultra-fine W-Y2O3 powder and using cold isostatic pressing and sintering technology, the problems of poor formability and large shrinkage in large-size block molding are solved, and W-Y2O3 powder with high density and good uniformity is achieved. Preparation of /W-Y2O3 bulk materials.
Patent Information
- Application Number
- CN202410782405.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
AI Technical Summary
Existing ultra-fine W-Y2O3 powder has problems such as poor formability, large shrinkage of the sintered body, dark cracks, and inability to form during the large-size block molding process, mainly due to large particle size differences, irregular morphology, and bulk density. Low.
A three-dimensional mixer is used to dry-mix pure tungsten powder and W-Y2O3 powder, and a high-density and high-strength W/W-Y2O3 green body is prepared through cold isostatic pressing, and low-temperature hydrogen pre-sintering and high-temperature argon gas are used After sintering, a W/W-Y2O3 bulk material with higher density and better uniformity is prepared.
It improves the powder properties of W-Y2O3 powder and the compressibility of large-size blocks, enhances the density and flexural strength of the green body, reduces the shrinkage of the sintered body, and achieves higher density and uniform W/W -Preparation of Y2O3 bulk materials.
Smart Images

Figure CN118768565A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultrafine powder pressing and sintering, and in particular to a preparation method for improving the compressibility of ultrafine W-Y2O3 powder large-size blocks by adding W powder. Background Art
[0002] Tungsten with high atomic number is considered to be the most promising plasma-facing material in IETR devices due to its high melting point, high thermal conductivity, low physical sputtering rate, low swelling and neutron damage resistance. However, the high ductile-brittle transition temperature, low recrystallization temperature and irradiation embrittlement limit the application of tungsten-based alloys. W-Y2O3 alloy has excellent mechanical properties, thermal shock damage resistance and radiation damage resistance, so the addition of nano-oxide (Y2O3) particles into the W matrix is considered to be one of the most promising candidate materials for future fusion reactors (PFM).
[0003] At present, the wet chemical method + spray drying method is mainly used to prepare ultrafine W-Y2O3 composite powder in large quantities. However, due to the limitation of the preparation process and the addition of the second phase Y2O3, the particle size difference of this powder is large (0.5-2μm), the morphology is extremely irregular, and the loose density and tap density are low, which leads to poor formability of the green body and large shrinkage of the sintered body. Especially for the forming of large-sized blocks, the formed body is prone to dark cracks and even cannot be formed. Therefore, how to improve the compressibility of large-sized blocks of ultrafine tungsten powder W-Y2O3 is a major challenge. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a preparation method for improving the compressibility of large-size blocks of ultrafine W-Y2O3 powder by adding W powder, and adopts a three-dimensional mixer to dry-mix pure tungsten powder and W-Y2O3 powder in a certain proportion, so as to improve the powder properties of W-Y2O3 powder, and then cold isostatic pressing is used to press out W / W-Y2O3 green bodies with high density and high strength, and then low-temperature hydrogen is used to pre-sinter W / W-Y2O3 pre-sintered blocks similar to green bodies, and finally high-temperature argon sintering is used to prepare W / W-Y2O3 block materials with high density and good uniformity.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is: A preparation method for improving the compressibility of large-sized blocks of ultrafine W-Y2O3 powder by adding W powder, firstly, a proper amount of W powder is mixed into the Y2O3 powder material to improve the powder properties of the W-Y2O3 powder; then, the powder in the rubber sleeve is uniformly pressurized in all directions by a cold isostatic press, and then a W / W-Y2O3 green body with high density and high strength is pressed out; then, a W / W-Y2O3 pre-sintered block similar to the green body is obtained by low-temperature hydrogen pre-sintering, so that the green body does not shrink, and only has slight diffusion at the point contact position between particles, and has a certain strength; finally, the W / W-Y2O3 material prepared by high-temperature argon sintering shows high density, strength and good uniformity.
[0006] As a preferred technical solution of the present invention, the particle size of the added W powder is 2-3 μm, the particle size of the W-Y2O3 powder is 0.5-2 μm, and the amount of W powder added is 20-30% of the mass of the W-Y2O3 powder. The preparation steps are as follows: Step 1: Preparation of W / W-Y2O3 powder Weigh W powder and W-Y2O3 powder according to a certain mass ratio, put them into a three-dimensional mixer and mix them for 12-24 hours to obtain W / W-Y2O3 powder; Step 2: Preparation of W / W-Y2O3 green body Then, an appropriate amount of uniformly mixed W / W-Y2O3 powder is weighed and pressed into a bag, compacted, sealed and vacuumed, and then placed in a cold isostatic press for cold isostatic pressing to obtain a W / W-Y2O3 green body; Step 3: Low temperature hydrogen pre-sintering The green body is subjected to hydrogen sintering at low temperature, the block is placed in a sintering boat, the sintering boat is then placed in a tubular furnace, the tubular furnace is evacuated, hydrogen is introduced, the temperature is increased for sintering for a period of time, and then the furnace is cooled to room temperature to obtain a W / W-Y2O3 pre-sintered block with a certain strength and no shrinkage; Step 4: High temperature argon sintering The W / W-Y2O3 pre-sintered block with certain strength and no shrinkage is sintered in argon at high temperature, and the block is placed on a graphite plate, and then the graphite plate is placed in a graphite furnace. The graphite furnace is evacuated, and then argon is introduced. The temperature is increased and sintered for a period of time, and then the furnace is cooled to room temperature to obtain a W / W-Y2O3 block material.
[0007] As a further preferred technical solution of the present invention, in the preparation method: The package used in step 2 is made of rubber and has a size of ø50×50 mm. The pressing pressure selected for cold isostatic pressing is 250-300 MPa, and the pressure is maintained for 3-5 minutes, and then the pressure is slowly released to remove the W / W-Y2O3 green body from the package.
[0008] Step 3: Low-temperature hydrogen pre-sintering. The specific steps are: hydrogen sintering the green body at low temperature, placing the block in a sintering boat, and then placing the sintering boat in a tubular furnace, evacuating the tubular furnace, then introducing hydrogen, and then heating to 1000-1200°C at 5-10°C / min, keeping warm for 1-2h, and then reducing the temperature to 480-520°C at 5°C / min, and then cooling to room temperature with the furnace to obtain a W / W-Y2O3 pre-sintered block with certain strength and no shrinkage.
[0009] Step 4: High-temperature argon sintering. The specific steps are as follows: argon sinter the W / W-Y2O3 pre-sintered block with a certain strength and no shrinkage at high temperature, place the block on a graphite plate, then place the graphite plate in a graphite furnace, evacuate the graphite furnace, then introduce argon, and then increase the temperature to 2000°C at 10°C / min, increase the temperature to 2150-2300°C at 5°C / min, keep warm for 3-4h, then reduce the temperature to 1000-880°C at 10°C / min, and then cool to room temperature with the furnace to obtain the W / W-Y2O3 block material.
[0010] The W / W-Y2O3 block material prepared by the present invention can successfully prepare a ø50×50cm block with good compressibility. Compared with the unimproved W-Y2O3 block material, the relative density of the green body can be increased by about 7%, and the bending strength of the pre-sintered block can be increased by about 37%. Compared with the prior art, the beneficial effects of the present invention are mainly manifested in: 1. The present invention improves the properties of W-Y2O3 powder and increases the loading capacity. After the pure tungsten powder and W-Y2O3 with poor powder properties are fully and evenly mixed by a three-dimensional mixer, some fine particles are filled in the gaps of coarse particles, thereby increasing the powder density; and the tungsten powder with narrow particle size distribution and high purity has good fluidity, so that the fluidity of the W-Y2O3 powder after mixing is also improved.
[0011] 2. The present invention improves the compressibility of W-Y2O3 green bodies of larger sizes. Using a cold isostatic press to compress large-sized, difficult-to-form powders can greatly reduce the structural differences between the outer and core parts of the bulk material and improve its uniformity. During the pressing process, the pressure is slowly increased, so that the fine powder and the coarse powder can flow fully and fill the internal voids better. The high pressure is maintained for a long time to fully transfer the pressure to the core, and the pressure is slowly released to prevent gas rebound, thereby improving the density and bending strength of the W-Y2O3 green body. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 a, b, c, d, e and f are SEM morphology images of the unproportioned W-Y2O3 powder of Example 1 and the W / W-Y2O3 powder proportioned with pure tungsten powder of Examples 2, 3, 4, 5 and 6, respectively.
[0013] Figure 2a, b, c, d, e and f are SEM morphology images of the fracture surfaces of the W-Y2O3 green body prepared without proportioning in Example 1 and the W / W-Y2O3 green body prepared by proportioning with pure tungsten powder in Examples 2, 3, 4, 5 and 6, respectively.
[0014] Figure 3 They are the relative densities of the W-Y2O3 green body prepared without proportioning in Example 1 and the W / W-Y2O3 green body prepared by proportioning with pure tungsten powder in Examples 2, 3, 4, 5, and 6.
[0015] Figure 4 They are the flexural strengths of the W-Y2O3 pre-sintered block prepared without proportioning in Example 1 and the W / W-Y2O3 pre-sintered block prepared by proportioning with pure tungsten powder in Examples 2, 3, 4, 5, and 6.
[0016] Figure 5 a, b, and c are the pore size distribution diagrams of W / W-Y2O3 pre-sintered blocks prepared by mixing pure tungsten powder of different particle sizes with examples 5, 2, and 6, respectively.
[0017] Figure 6 They are the relative densities of the final sintered block of W-Y2O3 prepared without proportioning in Example 1 and the final sintered block of W / W-Y2O3 prepared by proportioning with pure tungsten powder in Examples 2, 3, 4, 5, and 6. DETAILED DESCRIPTION
[0018] The present invention proposes a preparation method for improving the compressibility of large-sized blocks of ultrafine W-Y2O3 powder by adding W powder. First, a proper amount of W powder is mixed into the Y2O3 powder material to improve the powder properties of the W-Y2O3 powder; then, the powder in the rubber sleeve is uniformly pressurized in all directions by a cold isostatic press, and then a W / W-Y2O3 green body with high density and high strength is pressed out; then, a W / W-Y2O3 pre-sintered block similar to the green body is obtained by pre-sintering with low-temperature hydrogen, so that the green body does not shrink, and only has slight diffusion at the point contact position between particles, and has a certain strength; finally, the W / W-Y2O3 material prepared by high-temperature argon sintering exhibits higher density, strength and better uniformity. The present invention is further described in detail below in conjunction with the embodiments and drawings. Example 1
[0019] A method for preparing a relatively large-sized W-Y2O3 bulk material comprises the following steps: Step 1: Preparation of W-Y2O3 powder The W-Y2O3 powder prepared by wet chemical method-spray drying-hydrogen reduction is sieved with a sieve to remove plate crystals and impurities brought by the powder preparation process. The selected sieve size is 100-200 mesh. Figure 1As shown in (a), the particle size of the unproportioned W-Y2O3 powder is approximately 0.5μm-2μm, with a wide distribution, a large proportion of nano-scale small particles, severe agglomeration, and irregular particle shape.
[0020] Step 2: Preparation of W-Y2O3 green body Then weigh 420g of W-Y2O3 powder, manually vibrate and press it into a rubber sleeve of ø50×50mm, cover the plug, and then fix the sleeve filled with W-Y2O3 powder on the HY-100 tap density meter for vibration, with a single vibration frequency of 5000; wrap the uniformly vibrated sleeve with 2 layers of plastic wrap, and then use a vacuum sealing bag to evacuate and seal; then place the sealed sleeve in a cold isostatic press for cold isostatic pressing, the selected pressing pressure is 300MPa, the pressure is maintained for 5min, and then the pressure is slowly released to take the W-Y2O3 green body out of the sleeve. The fracture of the W-Y2O3 green body is as follows Figure 2 As shown in (a), due to the presence of Y2O3 impurities, the agglomeration of nano-tungsten particles and the irregular morphology of the powder make the green body have poor fluidity and many large pores. The green body density is only 10.57g / cm 3 ( Figure 3 as shown).
[0021] Step 3: Low temperature hydrogen pre-sintering The green body was hydrogen sintered at low temperature, and the block was placed in a sintering boat, and then the sintering boat was placed in a tube furnace. The tube furnace was evacuated, and then hydrogen was introduced. The temperature was raised to 1200℃ at 5℃ / min, kept at this temperature for 2h, and then dropped to 500℃ at 5℃ / min. Then, the W-Y2O3 pre-sintered block was obtained. The flexural strength of the W-Y2O3 pre-sintered block is only 113.7MPa ( Figure 4 as shown).
[0022] Step 4: High temperature argon sintering The W-Y2O3 pre-sintered block was sintered in argon at high temperature, and the block was placed on a graphite plate, and then the graphite plate was placed in a graphite furnace. The graphite furnace was evacuated, and then argon was introduced. The temperature was then raised to 2000°C at 10°C / min, and then raised to 2150°C at 5°C / min, and kept at this temperature for 3h. The temperature was then lowered to 1000°C at 10°C / min, and then cooled to room temperature with the furnace. The W-Y2O3 block material was obtained, and the relative density was only 75% ( Figure 6 as shown). Example 2
[0023] A method for preparing a high-compressibility W / W-Y2O3 bulk material having an optimal particle size ratio with tungsten powder comprises the following steps: Step 1: Preparation of W / W-Y2O3 powder The W-Y2O3 powder prepared by wet chemical method-spray drying-hydrogen reduction has a particle size distribution of 0.5-2μm. It is sieved with a sieve with a 100-mesh size. W powder and W-Y2O3 powder are weighed according to a certain mass ratio and loaded into a powder mixing tank. The powder mixing tank is then placed in a three-dimensional mixer and mixed for 24 hours to obtain about 595g of mixed powder. The specific working parameters of the mixer depend on the model. The morphology of W (2μm) / W-Y2O3 after sufficient mixing is as follows: Figure 1 As shown in (b), the proportion of nano-scale tungsten powder in the powder is reduced, which reduces the degree of agglomeration, and the volume ratio of larger-sized W particles to nano-scale W particles is about 7:3, which is conducive to filling pores. In addition, since the density of W (2μm) powder is relatively high, the density of the powder is increased.
[0024] In step 1, the particle size of the W powder in the powder mixing tank is 2 μm, the mass is 120 g, and the mass of the W-Y2O3 powder is 480 g.
[0025] Step 2: Preparation of W / W-Y2O3 green body Then weigh 520g of uniformly mixed W / W-Y2O3 powder, manually vibrate and press it into a rubber sleeve of ø50×50mm, cover the plug, and then fix the sleeve filled with W / W-Y2O3 powder on the HY-100 tap density meter for vibration, with a single vibration frequency of 5000; wrap the uniformly vibrated sleeve with 2 layers of plastic wrap, and then use a vacuum sealing bag to evacuate and seal; then place the sealed sleeve in a cold isostatic press for cold isostatic pressing, the selected pressing pressure is 300MPa, the pressure is maintained for 5min, and then the pressure is slowly released to take the W / W-Y2O3 green body out of the sleeve. The fracture of the W / W-Y2O3 green body is as follows Figure 2 As shown in (b), the pores of the 2 μm tungsten particles are filled, the pores in the W / W-Y2O3 green body are significantly reduced, and the pore size distribution is more uniform, so the green body density reaches 11.3 g / cm 3 ( Figure 3 as shown).
[0026] Step 3: Low temperature hydrogen pre-sintering The green body is hydrogen sintered at low temperature, and the block is placed in a sintering boat, and then the sintering boat is placed in a tube furnace. The tube furnace is evacuated, and then hydrogen is introduced. The temperature is then raised to 1200°C at 5°C / min, kept at this temperature for 2 hours, and then lowered to 500°C at 5°C / min. Then, the temperature is cooled to room temperature with the furnace, and a W / W-Y2O3 pre-sintered block with certain strength and no shrinkage is obtained. The flexural strength of the W / W-Y2O3 pre-sintered block reaches 155.9MPa ( Figure 4 In addition, Figure 5(b) The pore size distribution of the sintered block is 0.15-0.5um, the pore size is small, and the difference in pore size distribution between the inner and outer pores is small. Therefore, the W / W-Y2O3 material mixed with pure W powder exhibits higher pressing performance.
[0027] Step 4: High temperature argon sintering The W / W-Y2O3 pre-sintered block with certain strength and no shrinkage was sintered in argon at high temperature, and the block was placed on a graphite plate, and then the graphite plate was placed in a graphite furnace. The graphite furnace was evacuated, and then argon was introduced. The temperature was then raised to 2000°C at 10°C / min, and then raised to 2150°C at 5°C / min, and kept at this temperature for 3h, and then dropped to 1000°C at 10°C / min, and then cooled to room temperature with the furnace, and the W / W-Y2O3 block material was obtained, and the relative density was 93%, which was greatly improved ( Figure 6 as shown). Example 3
[0028] In this example, for comparison, the ratio of W to W-Y2O3 is changed to prepare W / W-Y2O3 bulk material.
[0029] The only difference between this embodiment and embodiment 2 is that the ratio adopted in step 1 for preparing W / W-Y2O3 powder is: the mass of W powder is 60g, and the mass of W-Y2O3 powder is 540g.
[0030] Step 1: The morphology of W (2 μm) / W-Y2O3 powder after full mixing is as follows: Figure 1 As shown in (c), the proportion of nano-scale tungsten powder in the powder has not changed significantly, and its powder morphology is similar to that of W-Y2O3 powder itself, so the pore filling effect is not obvious. However, due to the higher density of W (2μm) powder, the density of the mixed powder will also be improved.
[0031] The fracture surface of the W / W-Y2O3 green body prepared in step 2 is as follows: Figure 2 As shown in (c), it can be seen that the pores in the W / W-Y2O3 green body have not been significantly reduced. This is because the content of larger tungsten particles is small, and the pores between them cannot be well filled with nano-tungsten particles. However, because the density of W (2μm) powder is higher, the green body density can reach 11.22g / cm 3 ( Figure 3 as shown).
[0032] The W / W-Y2O3 pre-sintered block prepared in step 3 has a small proportion of W (2μm) powder, so the flexural strength of the W / W-Y2O3 pre-sintered block is not significantly improved, which is 142.5MPa ( Figure 4 as shown). Example 4
[0033] In this example, for comparison, the ratio of W to W-Y2O3 is changed to prepare W / W-Y2O3 bulk material.
[0034] The only difference between this embodiment and embodiment 2 is that the ratio adopted in step 1 for preparing W / W-Y2O3 powder is: the mass of W powder is 240g, and the mass of W-Y2O3 powder is 360g.
[0035] Step 1: The morphology of W (2 μm) / W-Y2O3 powder after full mixing is as follows: Figure 1 As shown in (d), the proportion of nano-scale tungsten powder in the powder changes significantly. In this ratio, the 2μm tungsten powder accounts for too much, and the nano-scale tungsten powder cannot fill the pores. However, due to the higher density of W (2μm) powder, the density of the mixed powder will also be improved.
[0036] The fracture surface of the W / W-Y2O3 green body prepared in step 2 is as follows: Figure 2 As shown in (d), it can be seen that the proportion of tungsten powder in the W / W-Y2O3 green body is too high, the filling of nano-tungsten particles is not enough to fill the pores, and the performance of W (2μm) block is not as good as that of W-Y2O3 block. Therefore, it is not advisable to add a large amount of W (2μm) powder. However, because the density of W (2μm) powder is higher, the green body density can reach 11.32g / cm 3 ( Figure 3 as shown).
[0037] In the W / W-Y2O3 pre-sintered block prepared in step 3, micro cracks have appeared on the fracture of the green body due to the large proportion of W (2μm) powder. Figure 2 As shown in the upper right corner of (d), the flexural strength of the W / W-Y2O3 pre-sintered block is only 114.9MPa ( Figure 4 as shown). Example 5
[0038] In this example, as a comparison, the particle size of W powder is changed to prepare W / W-Y2O3 bulk material.
[0039] The only difference between this embodiment and embodiment 2 is that the particle size of the W powder used in step 1 to prepare W / W-Y2O3 powder is 0.5 μm.
[0040] Step 1: The morphology of W (0.5 μm) / W-Y2O3 powder after full mixing is as follows: Figure 1 As shown in (e), the effect of a small amount of fine particles filling larger W-Y2O3 particles is achieved, thereby increasing the density of the mixed powder. However, as shown in the SEM morphology, even after sufficient mixing, the ultrafine 0.5μm tungsten powder is severely agglomerated, and the W-Y2O3 powder itself is also severely agglomerated, so the ideal filling effect cannot be achieved.
[0041] The fracture surface of the W / W-Y2O3 green body prepared in step 2 is as follows: Figure 2 As shown in (e), due to the large specific surface area and serious agglomeration of 0.5 μm powder, it is impossible to fully fill the voids of W-Y2O3 particles, which not only makes the fluidity worse during the pressing process, but also causes uneven pore distribution. Therefore, the maximum green density can only reach 11.28 g / cm 3 ( Figure 3 as shown).
[0042] The W / W-Y2O3 pre-sintered block prepared in step 3 has a maximum flexural strength of only 66.8MPa ( Figure 4 In addition, Figure 5 The pore size distribution of the pre-burned block shown in (a) is 0.2-0.7um. Although the pore size is small, the difference in pore size distribution inside and outside is large, which is very unfavorable for subsequent high-temperature sintering and easily causes uneven structure inside and outside the block. Example 6
[0043] In this example, as a comparison, the particle size of W powder is changed to prepare W / W-Y2O3 bulk material.
[0044] The only difference between this embodiment and embodiment 2 is that the particle size of the W powder used in step 1 to prepare W / W-Y2O3 powder is 5 μm.
[0045] Step 1: The morphology of W (5 μm) / W-Y2O3 powder after full mixing is as follows: Figure 1 As shown in (f), due to the small content of large particles of 5μm, they cannot be evenly distributed in the W-Y2O3 powder, so the smaller W-Y2O3 powder cannot fill the voids of the W (5μm) powder better. However, since the density of W (5μm) powder is significantly higher, the density of W (5μm) / W-Y2O3 powder will also be improved.
[0046] The fracture surface of the W / W-Y2O3 green body prepared in step 2 is as follows: Figure 2 As shown in (f), due to the small proportion of 5μm tungsten powder, the compact is not only unevenly distributed, but also the larger gaps between the larger tungsten particles cannot be well filled. The pore size distribution is as follows: Figure 3 As shown in the figure, this larger pore will become the flow channel of Y2O3 during high temperature sintering, causing Y2O3 to aggregate and significantly reduce performance. However, due to the significantly higher density of W (5μm) powder, the green density of W (5μm) / W-Y2O3 can reach 11.52g / cm 3 ( Figure 3 as shown).
[0047] The W / W-Y2O3 pre-sintered block prepared in step 3 has a flexural strength of 137.8MPa ( Figure 4 In addition, Figure 5 As shown in (c), the pore size distribution of the pre-sintered block is mainly between 0.5 and 1.2 um. The pore size distribution is uniform, but the size is relatively large. Such large pores are difficult to densify even through subsequent high-temperature sintering, and the larger the pore size, the more conducive it is to the flow and aggregation of Y2O3, which is not conducive to the performance of the final block.
[0048] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing ultrafine W-Y2O3 powder by adding W powder to improve the compressibility of large-sized blocks, characterized in that: Firstly, a proper amount of W powder is mixed into the Y2O3 powder material to improve the powder properties of the W-Y2O3 powder; then, the powder in the rubber sleeve is uniformly pressurized in all directions by a cold isostatic press to press out a W / W-Y2O3 green body with high density and high strength; then, a W / W-Y2O3 pre-sintered block similar to the green body is obtained by low-temperature hydrogen pre-sintering, so that the green body does not shrink, and only has slight diffusion at the point contact parts between particles, and has a certain strength; finally, the W / W-Y2O3 material prepared by high-temperature argon sintering exhibits higher density, strength and better uniformity.
2. The preparation method according to claim 1, characterized in that The particle size of the added W powder is 2-3 μm, the particle size of the W-Y2O3 powder is 0.5-2 μm, and the amount of W powder added is 20-30% of the mass of the W-Y2O3 powder.
3. The preparation method according to claim 1 or 2, characterized in that: Here are the steps: Step 1: Preparation of W / W-Y2O3 powder Weigh W powder and W-Y2O3 powder according to a certain mass ratio, put them into a three-dimensional mixer and mix them for 12-24 hours to obtain W / W-Y2O3 powder; Step 2: Preparation of W / W-Y2O3 green body Then, an appropriate amount of uniformly mixed W / W-Y2O3 powder is weighed and pressed into a bag, compacted, sealed and vacuumed, and then placed in a cold isostatic press for cold isostatic pressing to obtain a W / W-Y2O3 green body; Step 3: Low temperature hydrogen pre-sintering The green body is subjected to hydrogen sintering at low temperature, the block is placed in a sintering boat, the sintering boat is then placed in a tubular furnace, the tubular furnace is evacuated, hydrogen is introduced, the temperature is increased for sintering for a period of time, and then the furnace is cooled to room temperature to obtain a W / W-Y2O3 pre-sintered block with a certain strength and no shrinkage; Step 4: High temperature argon sintering The W / W-Y2O3 pre-sintered block with certain strength and no shrinkage is sintered in argon at high temperature, and the block is placed on a graphite plate, and then the graphite plate is placed in a graphite furnace. The graphite furnace is evacuated, and then argon is introduced. The temperature is increased and sintered for a period of time, and then the furnace is cooled to room temperature to obtain a W / W-Y2O3 block material.
4. The preparation method according to claim 3, characterized in that: The material of the package used in step 2 is rubber and the size is 5. The preparation method according to claim 3, characterized in that: In step 2, the pressing pressure selected for cold isostatic pressing is 250-300 MPa, the pressure is maintained for 3-5 minutes, and then the pressure is slowly released to take the W / W-Y2O3 green body out of the package.
6. The preparation method according to claim 3, characterized in that: Step 3: Low temperature hydrogen pre-sintering: The green body is hydrogen sintered at low temperature, the block is placed in a sintering boat, and then the sintering boat is placed in a tubular furnace. The tubular furnace is evacuated, and then hydrogen is introduced. The temperature is then raised to 1000-1200°C at 5-10°C / min, kept for 1-2h, and then dropped to 480-520°C at 5°C / min. Subsequently, the W / W-Y2O3 pre-sintered block with certain strength and no shrinkage is obtained.
7. The preparation method according to claim 3, characterized in that: Step 4 High temperature argon sintering The specific steps are: The W / W-Y2O3 pre-sintered block with certain strength and no shrinkage is sintered in argon at high temperature, the block is placed on a graphite plate, and then the graphite plate is placed in a graphite furnace. The graphite furnace is evacuated, and then argon is introduced. The temperature is then increased to 2000°C at 10°C / min, and then increased to 2150-2300°C at 5°C / min, and kept warm for 3-4h, and then decreased to 1000-880°C at 10°C / min, and then cooled to room temperature with the furnace to obtain a W / W-Y2O3 block material.
8. The W / W-Y2O3 bulk material prepared by the method according to any one of claims 1 to 7.