Oxygen carrier for preparing synthesis gas through methane chemical chain reforming as well as preparation method and application of oxygen carrier
By using the perovskite structure PrxLa1-xCoyFe1-yO3 oxygen carrier in methane chemical chain reforming technology, the problems of low methane conversion rate and poor cycle stability of the oxygen carrier are solved, and efficient methane conversion and synthesis gas generation are achieved. , suitable for high temperature chemical chain reactions.
Patent Information
- Application Number
- CN202410945241.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
The methane conversion rate of the oxygen carrier in the existing methane chemical chain reforming technology is low and the cycle stability is poor, resulting in high energy consumption and poor syngas quality.
The perovskite-structured PrxLa1-xCoyFe1-yO3 oxygen carrier is prepared through the sol-gel method. Pr and Co ions are introduced to improve the dispersion and oxygen transmission rate of the oxygen carrier and maintain stability in high-temperature cycling environments.
It significantly improves the methane conversion rate and synthesis gas yield, ensures the cycle stability and sintering resistance of the oxygen carrier, is suitable for high-temperature chemical chain reactions, and produces excellent synthesis gas quality.
Smart Images

Figure CN118771306A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of preparing synthesis gas by chemical loop reforming of methane, and in particular relates to an oxygen carrier used for preparing synthesis gas by chemical loop reforming of methane, and a preparation method and application thereof. Background Art
[0002] Methane dry reforming (CH4+CO2→2CO+2H2, ΔH 0 298K =247kJ / mol) can convert methane and carbon dioxide into industrially important synthesis gas, but the reaction is highly endothermic, energy-intensive, and easily forms carbon deposits covering the active sites, causing catalyst deactivation; in addition, the hydrogen-carbon ratio of the generated synthesis gas is about 1. If subsequent methanol synthesis or Fischer-Tropsch synthesis (the required H2 / CO ratio is 2) is to be carried out, a gas adjustment process needs to be added, which increases energy consumption. Methane chemical chain reforming technology uses oxygen carriers (usually metal oxides, MO) to circulate between the fuel reactor and the regeneration reactor to decouple the gas-gas reaction into two gas-solid half-reactions (CH4+MO=2H2+CO, CO2+M=MO+CO), which can not only produce synthesis gas with an H2 / CO ratio of 2, which can be directly used as the feed gas for subsequent methanol synthesis or Fischer-Tropsch synthesis, but also convert greenhouse gases into CO; if CO2 is replaced by H2O (H2O+M=MO+H2), high-purity hydrogen without carbon pollution can also be obtained; if CO2 and H2O are simultaneously introduced into the regeneration reactor, additional synthesis gas can be obtained. The key to the successful operation of methane chemical looping reforming technology lies in the development of oxygen carriers that are resistant to high temperatures and have excellent performance.
[0003] At present, the research on chemical chain oxygen carriers mainly focuses on transition metal oxide oxygen carriers and composite metal oxide oxygen carriers. Iron-based oxygen carriers are considered to be one of the ideal oxygen carrier materials because of their low cost, environmental friendliness, high oxygen carrying capacity, and good reaction activity with CO2 or water vapor.
[0004] Dai et al. [J. Phys. Chem. B, 2006, 110, 45, 22525-22531] studied three iron-based perovskite oxides AFeO3 (A = La, Nd, Eu) for partial oxidation of methane to produce synthesis gas by chemical chaining, and found that LaFeO3 showed the best synthesis gas yield due to its high oxygen mobility. However, the reaction activity of pure LaFeO3 oxygen carrier with methane is not high (methane conversion rate is about 60-70%), and the cycle stability is poor.
[0005] At present, the application of methane chemical chain reforming technology to Fe-based perovskite oxygen carriers still has problems such as low methane conversion rate. Summary of the invention
[0006] In order to overcome the problem of low methane conversion rate in the prior art, the purpose of the present invention is to provide an oxygen carrier for methane chemical loop reforming to produce synthesis gas and its preparation method and application, the oxygen carrier has higher methane conversion rate, higher synthesis gas yield and excellent cycle stability, the synthesis route is short, and it is easy to promote.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] An oxygen carrier for methane chemical loop reforming to produce synthesis gas, the oxygen carrier having a perovskite structure, the chemical formula of which is Pr x La 1-x Co y Fe 1-y O3, where 0 <x≤1,0≤y≤1。
[0009] Furthermore, x is 0.1, 0.2, 0.4, 0.6 or 0.8, and y is 0.1, 0.3, 0.5, 0.7 or 0.9.
[0010] A method for preparing an oxygen carrier for producing synthesis gas through chemical loop reforming of methane comprises the following steps:
[0011] Press Pr x La 1-x Fe y Co 1-y O3, dissolving the precursor of Pr, the precursor of La, the precursor of Co and the precursor of Fe in hot water to form a precursor solution; wherein, 0 <x≤1,0≤y≤1;
[0012] Add a hot citric acid aqueous solution to a precursor solution, then add ethylene glycol or isopropanol, stir under heating conditions until it is in a gel state, dry, calcine, and shape to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0013] Furthermore, the precursor of Pr is at least one of Pr(NO3)3·6H2O, Pr(CH3COO)3·xH2O and Pr2(SO4)3·8H2O; the precursor of La is at least one of La(NO3)3·6H2O and La(CH3COO)3·xH2O; the precursor of Fe is at least one of FeCl3, Fe(NO3)3·9H2O and FeSO4; the precursor of Co is at least one of Co(NO3)2·6H2O and Co(CH3COO)2·4H2O.
[0014] Furthermore, the total concentration of the Pr precursor, the La precursor, the Co precursor and the Fe precursor in the precursor solution is 0.9 to 1.5 mol / L.
[0015] Furthermore, the amount of citric acid used is 1.5 to 2.5 times the total molar amount of Pr, La, Co and Fe ions.
[0016] Furthermore, the amount of ethylene glycol or isopropanol used is 0.5-1.2% of the total volume of the precursor solution and the citric acid solution.
[0017] Furthermore, the specific process of calcination is: first calcining at 300-500°C for 2-5h, and then calcining at 800-1000°C for 2-5h.
[0018] An application of an oxygen carrier in methane chemical loop reforming to produce synthesis gas, characterized in that the oxygen carrier circulates between two connected fuel reactors and a regeneration reactor; wherein, in the fuel reactor, the oxygen carrier oxidizes methane at 700-1000° C. to produce synthesis gas; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 700-1000° C. in an oxidizing atmosphere;
[0019] The fuel reactor contains a mixture of methane and inert gas.
[0020] Furthermore, the oxidizing atmosphere is a mixture of any one of carbon dioxide, oxygen, water vapor and an inert gas, or the oxidizing atmosphere is a mixture of water vapor and carbon dioxide;
[0021] The volume fraction of methane in the mixture of methane and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of carbon dioxide and inert gas, the volume fraction of carbon dioxide in the mixture of carbon dioxide and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of water vapor and inert gas, the volume fraction of water vapor in the mixture of water vapor and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of oxygen and inert gas, the volume fraction of oxygen in the mixture of oxygen and inert gas is 1% to 100%.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The doping of Pr and Co in the oxygen carrier of the present invention does not lead to the formation of impurity phase. 3+ 、Co 2+ ions partially replaced La 3+ , Fe 3+ Entering the perovskite lattice, forming Pr x La 1-x Co y Fe 1-yThe composite perovskite structure of O3. Pr and Co ion substitution not only reduces the grain size, improves the dispersibility of the oxygen carrier and the oxygen transfer rate, but also introduces new methane activation centers, improves the methane conversion rate, and the synergy of Pr and Co greatly improves the synthesis gas yield. The perovskite structure is not significantly damaged during multiple cycles. The prepared oxygen carrier has strong mechanical stability and anti-sintering ability during the methane chemical chain reforming cycle reaction, is suitable for high-temperature chemical chain environments, and has excellent cycle stability.
[0024] The oxygen carrier prepared by the present invention has excellent methane activation ability, synthesis gas yield and cycle stability. 3+ The methane conversion rate and syngas yield in the post-methane reduction process are improved without carbon deposition. 3+ The introduction of an appropriate amount of can effectively reduce the crystal size of the oxygen carrier, improve the dispersion of the metal and the diffusion and transmission rate of lattice oxygen. The introduction of Co generates single-state Co during the redox process, which greatly improves the methane activation ability. In addition, Co 2+ Partially replace Fe 3+ The resulting non-conservation of charge tends to increase the oxygen vacancy content of the oxygen carrier; the co-doping of Pr and Co allows the oxygen carrier to generate La2O3 rich in large cations in situ after multiple redox cycles, greatly improving the anti-sintering ability of the oxygen carrier. The Co element formed in situ after redox treatment is an important active site for methane activation, which matches the greater oxygen transfer rate after Pr doping, thereby efficiently activating methane and generating synthesis gas, the production of anti-sintering La2O3 and the maintenance of the perovskite structure, making the La2O3 after Pr and Co doping 0.8 Pr 0.2 Fe 0.7 Co 0.3 During 50 continuous cycles, the O3 oxygen carrier not only has high methane conversion rate (98.1-98.9%), CO selectivity (87.5-91.0%), H2 selectivity (85.8-89.7%), synthesis gas yield (2.35-2.54 mmol / g), and suitable H2 / CO ratio (1.92-1.96), but also exhibits excellent cycle stability.
[0025] The co-doping of Pr and Co in the present invention not only improves the methane catalytic activity of the oxygen carrier, but also increases the release rate of lattice oxygen and the anti-sintering performance of the oxygen carrier particles during the reaction, thereby improving the cycle stability. 0.2 La 0.8 Co 0.3 Fe 0.7O3 oxygen carrier has the best methane reaction activity. By the 50th cycle, the methane conversion rate is still higher than 98% and the syngas selectivity is maintained at about 90%. The molar ratio of H2 to CO is maintained at 1.9-2.0, close to the ideal value of 2, and the syngas quality is high. This shows that the oxygen carrier has excellent methane reaction activity, syngas yield and cycle stability.
[0026] Furthermore, the Pr having a perovskite structure in the present invention x La 1-x Co y Fe 1-y O3 composite metal oxides are universal in oxidizing atmospheres and can be oxidatively regenerated in air, water vapor, carbon dioxide or a water vapor / carbon dioxide mixture, and exhibit a cyclic stability similar to that of carbon dioxide reactions. The preparation route of this oxygen carrier is short, environmentally friendly, and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 X-ray powder diffraction spectra of fresh oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Example 1, Example 2;
[0028] Figure 2 The kinetic curve of the oxygen carrier prepared in Comparative Example 1 during the reaction process;
[0029] Figure 3 The kinetic curve diagram of the oxygen carrier prepared in Comparative Example 2 during the reaction process;
[0030] Figure 4 The kinetic curve of the oxygen carrier prepared in Example 1 during the reaction process;
[0031] Figure 5 The kinetic curve diagram of the oxygen carrier prepared in Example 2 during the reaction process;
[0032] Figure 6 A comparison chart of CH4 conversion rate and H2 / CO of oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Example 1, Example 2 during 10 cycles of reaction;
[0033] Figure 7 It is a schematic diagram of the synthesis gas yield of the oxygen carrier prepared in Comparative Example 1, Comparative Example 2 and Example 1, Example 2 during 10 cycles of reaction;
[0034] Figure 8 Schematic diagram of CH4 conversion rate, CO selectivity, H2 selectivity and H2 / CO of the oxygen carrier prepared in Example 2 during 50 cycles of reaction;
[0035] Fig. 9Schematic diagram of syngas yield of the oxygen carrier prepared in Example 2 during 50 cycles of reaction;
[0036] Fig.10 X-ray powder diffraction patterns of the oxygen carrier prepared in Example 1 in the fresh state and after 2 cycles and 10 cycles respectively;
[0037] Fig.11 X-ray powder diffraction patterns of the oxygen carrier prepared in Example 2 in the fresh state and after 2 cycles and 10 cycles respectively. Detailed implementation manners
[0038] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments, but the present invention is not limited to the following examples.
[0039] The oxygen carrier for chemical looping reforming of methane to syngas of the present invention is a composite metal oxide with a perovskite structure, and its structural general formula is Pr x La 1-x Co y Fe 1-y O3, where 0 < x ≤ 1, 0 ≤ y ≤ 1. Preferably, x is 0.1, 0.2, 0.4, 0.6 or 0.8, and y is 0.1, 0.3, 0.5, 0.7 or 0.9.
[0040] The preparation method of the oxygen carrier in the present invention includes the following steps:
[0041] Specifically, the oxygen carrier is prepared by the sol-gel method. First, Pr precursor, La precursor, Co precursor, and Fe precursor are added in a certain molar ratio and dissolved in deionized water at 60 °C to form a precursor solution. Citric acid particles are weighed and dissolved in hot deionized water, and the citric acid solution is poured into the precursor solution to form a mixed solution. Then, isopropanol or ethylene glycol is added dropwise to the mixed solution to disperse the solution, and the solution is continuously stirred until it becomes gel-like under heating conditions, dried, ground, calcined, and pressure-molded to obtain the oxygen carrier for chemical looping reforming of methane to syngas
[0042] The precursor of Pr is at least one of Pr(NO3)3·6H2O, Pr(CH3COO)3·xH2O and Pr2(SO4)3·8H2O; the precursor of La is at least one of La(NO3)3·6H2O and La(CH3COO)3·xH2O; the precursor of Fe is at least one of FeCl3, Fe(NO3)3·9H2O and FeSO4; the precursor of Co is Co(NO3)2·6H2O, Co(CH3COO)2·4 At least one of H2O; the total concentration of the precursors of Pr, La, Co and Fe in the precursor solution is 1-1.5 mol / L; the amount of citric acid required is 1.5-2.5 times the molar amount of the total metal cations in the solution; the amount of ethylene glycol or isopropanol used is 0.5-1.2% of the total volume of the precursor solution and the citric acid solution; the drying process is drying at 50-80°C for 8-12 hours; the calcination process is calcining at 300-500°C for 2-5 hours, and then calcining at 800-1000°C for 2-5 hours.
[0043] The oxygen carrier as described above is applied to the methane chemical loop reforming process, specifically, the oxygen carrier circulates between two interconnected reactors (a fuel reactor and a regeneration reactor); wherein, in the fuel reactor, the oxygen carrier oxidizes methane to produce synthesis gas; in the regeneration reactor, the oxygen carrier is oxidized and regenerated under an oxidizing atmosphere and enters the next cycle process; the reaction is carried out under normal pressure and the reaction temperature is 800-1000°C; the fuel reactor is a mixture of methane and inert gas, and the oxidizing atmosphere in the regeneration reactor is a mixture of carbon dioxide or oxygen or water vapor and inert gas or a mixture of water vapor and carbon dioxide and inert gas.
[0044] Among them, the volume fraction of methane in the mixture of methane and inert gas is 1% to 100%, the volume fraction of carbon dioxide in the mixture of carbon dioxide and inert gas is 1% to 100%, the volume fraction of water vapor in the mixture of water vapor and inert gas is 1% to 100%, and the volume fraction of oxygen in the mixture of oxygen and inert gas is 1% to 100%.
[0045] The oxygen carrier can effectively improve the reaction activity of the oxygen carrier and methane, and the methane conversion rate is as high as 98% or more. If carbon dioxide is used as the oxidizing atmosphere, the selectivity of the synthesis gas is above 86%. At the same time, it has excellent anti-carbon deposition performance, wherein H2 / CO is about 2, and can be directly used for Fischer-Tropsch synthesis. The oxygen carrier has excellent methane reaction activity and stability in multiple redox cycles. Among them, if water vapor, water / carbon dioxide is used as the oxidizing atmosphere, high-value-added products such as high-purity hydrogen, carbon monoxide or synthesis gas can also be produced.
[0046] Comparative Example 1
[0047] Preparation of LaFeO3 oxygen carrier
[0048] Weigh a certain molar ratio of La(NO3)3·6H2O and Fe(NO3)3·9H2O and dissolve them in 60℃ deionized water, continue heating and stirring. After they are completely dissolved, take another beaker and weigh a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) and stir to dissolve. At this time, pour the metal precursor solution with a concentration of 0.9-1.0mol / L into the citric acid solution. After the citric acid is fully dissolved, add a small amount of isopropanol dispersion solution. The specific amount of isopropanol dispersion solution is 0.5% of the total volume of the precursor solution. Then, place the mixed solution in a constant temperature water bath at 80℃ and stir to fully evaporate the water in the solution. The remaining porous viscous colloid is dried at 120℃ for 600 minutes to obtain a brown-yellow brittle precursor. Grind the precursor thoroughly, place the sample in a muffle furnace for calcination, first heat it to 500℃ at a heating rate of 10℃ per minute, and keep it for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 900°C at a heating rate of 10°C per minute and kept for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles under a pressure of 15 MPa to obtain an oxygen carrier for methane chemical loop reforming to produce synthesis gas.
[0049] Comparative Example 2
[0050] LaFe 0.7 Co 0.3 Preparation of O3 oxygen carrier
[0051] Weigh a certain amount of La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O in a molar ratio of 10:7:3 and dissolve them in 60℃ deionized water. Continue heating and stirring. After they are completely dissolved, take another beaker and weigh a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) and stir to dissolve. At this time, pour the metal precursor solution with a concentration of 0.9-1.0mol / L into the citric acid solution. After the citric acid is fully dissolved, add a small amount of isopropanol dispersion solution. The specific amount of isopropanol dispersion solution is 1.2% of the total volume of the precursor solution. Then, place the mixed solution in a constant temperature water bath at 80℃ and stir to fully evaporate the water in the solution. The remaining porous viscous colloid is dried at 120℃ for 600 minutes to obtain a yellow-brown brittle precursor. The precursor was fully ground and the sample was calcined in a muffle furnace, first heated to 500°C at a heating rate of 10°C per minute and retained for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 900°C at a heating rate of 10°C per minute and retained for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles at a pressure of 15MPa to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0052] Example 1
[0053] Pr 0.2 La 0.8 Preparation of FeO3 oxygen carrier
[0054] Weigh a certain amount of Pr(NO)3·6H2O, La(NO3)3·6H2O and Fe(NO3)3·9H2O in a molar ratio of 2:8:10 and dissolve them in 60℃ deionized water. Continue heating and stirring. After they are completely dissolved, weigh a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) in another beaker and stir to dissolve. At this time, pour the metal precursor solution with a concentration of 0.9mol / L into the citric acid solution. After the citric acid is fully dissolved, add a small amount of isopropanol dispersion solution. The specific amount of isopropanol dispersion solution is 1% of the total volume of the precursor solution. Then, place the mixed solution in a constant temperature water bath at 80℃ and stir to fully evaporate the water in the solution. The remaining porous viscous colloid is dried at 120℃ for 600 minutes to obtain a brown-yellow brittle precursor. The precursor was fully ground and the sample was calcined in a muffle furnace, first heated to 500°C at a heating rate of 10°C per minute and retained for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 900°C at a heating rate of 10°C per minute and retained for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles at a pressure of 15MPa to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0055] Example 2
[0056] Pr 0.2 La 0.8 Fe 0.7 Co 0.3 Preparation of O3 oxygen carrier
[0057] According to the molar ratio of 2:8:7:3, a certain mass of Pr(NO)3·6H2O, La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O were weighed and dissolved in 60℃ deionized water, and continued to heat and stir. After complete dissolution, a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) was weighed in another beaker and stirred to dissolve. At this time, the metal precursor solution with a concentration of 0.9mol / L was poured into the citric acid solution. After the citric acid was fully dissolved, a small amount of isopropanol dispersion solution was added dropwise, and the specific amount was 1% of the total volume of the precursor solution. After that, the mixed solution was placed in a constant temperature water bath at 80℃ and stirred to fully evaporate the water in the solution, and the remaining porous viscous colloid was dried at 120℃ for 600 minutes to obtain a yellow-brown brittle precursor. The precursor was fully ground and the sample was calcined in a muffle furnace, first heated to 500°C at a heating rate of 10°C per minute and retained for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 900°C at a heating rate of 10°C per minute and retained for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles at a pressure of 15MPa to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0058] Example 3 XRD test of oxygen carrier
[0059] The oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Examples 1 and 2 were tested by X'pert Pro Super type X-ray diffractometer, which was produced by PAN Analytical of the Netherlands. The copper target Kα line was used as the light source (λ=0.15432nm), the graphite monochromator, the tube voltage and the tube current were 40kV and 40mA respectively. The X-ray diffraction test results are shown in FIG. Figure 1 shown.
[0060] from Figure 1 It can be found that only the diffraction peak of the perovskite LaFeO3 phase can be observed in all oxygen carriers, and no impurity phase is produced, indicating that the oxygen carriers after calcination are all pure perovskite structures. With the addition of Pr (x = 0.2, y = 0), the LaFeO3 diffraction peak gradually shifts to a higher angle, and Pr 3+ Ionic radius Less than La 3+ Ionic radius Description 3+ Ions successfully replaced La 3+ ions enter the LaFeO3 lattice, forming Pr x La 1-x FeO3 structure. Pure Co 2+The addition of (x = 0, y = 0.3) also caused the LaFeO3 diffraction peak to shift to a higher angle, indicating the formation of LaCo y Fe 1-y O3 structure. 3+ and Co 2+ Co-doping (x = 0.2, y = 0.3) makes the LaFeO3 diffraction peak shift further to a higher angle, indicating that Pr 3+ and Co 2+ The ions all entered the LaFeO3 lattice, forming Pr x La 1-x Co y Fe 1-y O3 structure.
[0061] Compared with undoped LaFeO3 (x=0, y=0), the pure Pr doping (x=0.2, y=0) and Co 2+ of doping (x = 0, y = 0.3), and Pr 3+ and Co 2+ The co-doping of ions (x = 0.2, y = 0.3) broadens the LaFeO3 diffraction peak. From Table 1, we can see that the grain size of LaFeO3 decreases from 50nm in the x = 0, y = 0 sample to 38-42nm. The reason may be that the charge is not conserved (such as Co 2+ Partially replace Fe 3+ ), increase in surface defects (such as lattice distortion caused by ion radius mismatch), etc.
[0062] Table 1 XRD cell parameters and grain size comparison table of comparative example 1, comparative example 2, embodiment 1, embodiment 2
[0063]
[0064] Example 4 Activity Evaluation of Oxygen Carriers
[0065] The oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Example 1, Example 2 were evaluated for their activity in the methane chemical chain reforming reaction using a fixed bed reactor. The amount of oxygen carrier used was 300 mg, and the particle size was 20-40 mesh. The fuel gas composition was 5% CH4 / Ar, the flow rate was 15 ml / min, the reaction temperature was 900°C, the reaction time was 20 min, and the reaction pressure was normal pressure. The reactor outlet gas was analyzed online using a GAM-200 mass spectrometer. The reaction results are shown in Figure 2-Figure 5 shown.
[0066] like Figure 2As shown, a small amount of CO2 is generated by the LaFeO3 oxygen carrier at the beginning of the reaction, and a large amount of unreacted CH4 exists in the process. H2 and CO show a trend of first increasing and then slowly increasing in the whole process, indicating that the methane activity is low and the release rate of lattice oxygen is slow.
[0067] Compared with the pure LaFeO3 (x=0, y=0) in Comparative Example 1, the Co-doped LaFe 0.7 Co 0.3 O3(x=0、y=0.3, Figure 3 ) The unreacted methane content of the oxygen carrier decreased significantly, indicating that the introduction of Co greatly improved the methane catalytic activity of the oxygen carrier. When an appropriate amount of Pr was introduced to replace La (x = 0.2, y = 0, Figure 4 ), the unreacted CH4 content in the initial stage of the reaction (0-5min) was greatly reduced, and the rapid generation of synthesis gas CO and H2 was observed in the initial stage of the reaction (within 1min), and the synthesis gas yield was significantly increased. It can be seen that the appropriate amount of Pr addition mainly increased the release rate of lattice oxygen. When the appropriate amount of Pr and Co were co-substituted (x = 0.2, y = 0.3, Figure 5 ), not only is the unreacted CH4 content almost unobservable, but also a large amount of synthesis gas CO and H2 can be observed in ~4 minutes. It can be seen that the co-incorporation of Pr and Co not only improves the catalytic activity of methane but also increases the release rate of lattice oxygen. The main reason is that the incorporation of Pr mainly increases the mobility of lattice oxygen, and the incorporation of Co mainly increases the catalytic activity of methane. The two work together to make Pr 0.2 La 0.8 Co 0.3 Fe 0.7 O3 oxygen carrier takes into account high methane conversion rate, lattice oxygen mobility and high synthesis gas yield.
[0068] Example 5 Evaluation of the Cyclic Stability of Oxygen Carriers
[0069] The oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Example 1 and Example 2 were evaluated for the cyclic stability of the oxygen carrier methane chemical loop reforming using a fixed bed reactor, and the oxygen carrier prepared in Example 2 was further evaluated for the cyclic stability of the oxygen carrier methane chemical loop reforming using a fixed bed reactor. The amount of oxygen carrier was 300 mg, and the particle size was 20-40 mesh. The fuel gas composition was 5% CH4 / Ar, the flow rate was 15 ml / min, the reaction temperature was 900°C, and the reaction pressure was normal pressure. After 8 minutes of reduction, switch to Ar purging until the content of all gases in the reaction system except inert gas was less than 1000ppm, the flow rate was 30 ml / min, and then switch to an oxidizing atmosphere, the composition was 5% CO2 / Ar, the flow rate was 15 ml / min, the reaction temperature was 900°C, and the time was 10 min. The above steps were repeated 10 times to test the stability of the oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Examples 1 and 2, and the above steps were repeated 50 times to further test the stability of the oxygen carrier prepared in Example 2. The reactor outlet gas was analyzed online using a GAM-200 mass spectrometer. The results of the 10-cycle stability evaluation of the oxygen carriers prepared in Comparative Example 1, Comparative Example 2 and Examples 1 and 2 are as follows: Figure 6 , 7 As shown, the stability of the oxygen carrier prepared in Example 2 after 50 cycles is evaluated as follows: Figure 8 , 9 shown.
[0070] Depend on Figure 6 and Figure 7 It can be seen that LaFeO3 (x=0, y=0) oxygen carrier has the worst methane activity. After 10 cycles, the methane conversion rate dropped sharply from 85% to 52%. 0.8 Pr 0.2 After 10 cycles of FeO3 (x = 0.2, y = 0) oxygen carrier, the methane conversion rate dropped from 86% to 69%, and LaFe 0.7 Co 0.3 O3 (x = 0, y = 0.3) oxygen carrier has a strong methane activation ability. After 10 cycles, the methane conversion rate dropped from 95% to 84%. 0.8 Pr 0.2 Fe 0.7 Co 0.3 O3 (x = 0.2, y = 0.3) oxygen carrier has the strongest methane activation ability. During the 10 cycles, the methane conversion rate was maintained at around 99% and there was no downward trend. However, the oxygen carriers prepared in Comparative Example 1, Comparative Example 2, and Example 1 showed a significant decrease in methane conversion rate during the 10 cycles. It can be seen that La doped with Pr and Co 0.8 Pr 0.2 Fe 0.7 Co 0.3O3 oxygen carrier not only has high methane reaction activity and synthesis gas yield, but also has high cycle stability.
[0071] from Figure 8 and Fig. 9 It can be seen that after 50 cycles, the Pr and Co doped x = 0.2, y = 0.3 oxygen carrier still maintains a CH4 conversion rate of 98%, a CO selectivity of about 90.5%, a H2 selectivity of about 89.5%, a syngas yield of up to 2.52mmol / g, and H2 / CO is always maintained between 1.9 and 2.0. The above results show that the La doped with Pr and Co 0.8 Pr 0.2 Fe 0.7 Co 0.3 The O3 oxygen carrier exhibited excellent methane reaction activity, synthesis gas selectivity, synthesis gas yield and cycle stability during 50 consecutive high-temperature redox reactions. Its high cycle life demonstrates its great application potential.
[0072] Example 6 XRD test of oxygen carrier after cycling
[0073] XRD tests of fresh oxygen carriers and oxygen carriers after 2 and 10 cycles prepared in Example 1 and Example 2 were conducted on an X'pert Pro Super type X-ray diffractometer, which is produced by PAN Analytical of the Netherlands. The copper target Kα line is used as the light source (λ=0.15432nm), the graphite monochromator, the tube voltage and the tube current are 40kV and 40mA respectively. The X-ray diffraction test results are shown in FIG. Fig.10 , Fig.11 shown.
[0074] from Fig.10 and Fig.11 See La as Example 1 0.8 Pr 0.2 FeO3 (x = 0.2, y = 0) oxygen carrier showed no obvious structural changes during the cycle, and the perovskite structure was maintained. As the number of cycles increased, the diffraction peak shifted to the left, which may be related to the Fe 3+ ions and the formation of oxygen vacancies. 0.8 Pr 0.2 Fe 0.7 Co 0.3 After 10 cycles, the main phase of the O3 (x = 0.2, y = 0.3) oxygen carrier is still the perovskite phase, but after 10 cycles, La2O3 and single-phase Co phase appear. Due to thermodynamic limitations, Co cannot be oxidized by CO2 under the operating conditions described in Example 5, so the single-phase Co phase is maintained. Single-phase Co has a very strong methane activation ability, so that La2O3 and single-phase Co doped with Pr and Co can be used as the catalyst for the oxidation of Pr and Co.0.8 Pr 0.2 Fe 0.7 Co 0.3 The O3 oxygen carrier always maintained a methane conversion rate of more than 98% during 50 consecutive cycles. La2O3 rich in large cations can improve the anti-sintering ability of the oxygen carrier. In summary, the Co element formed in situ after redox treatment is an important active site for methane activation, which matches the greater oxygen transfer rate after Pr doping, thereby efficiently activating methane and generating synthesis gas, the production of anti-sintering La2O3 and the maintenance of the perovskite structure, making the La2O3 after Pr and Co doping more active. 0.8 Pr 0.2 Fe 0.7 Co 0.3 The O3 oxygen carrier not only has high methane conversion rate, synthesis gas yield and excellent cycle stability during 50 continuous cycles.
[0075] Example 7
[0076] The oxygen carrier prepared in Example 2 was evaluated for its activity in methane chemical looping reforming reaction using a fixed bed reactor. The evaluation procedure was the same as that in Example 4, except that the fuel gas composition was 5% O2 / Ar.
[0077] Example 8
[0078] The oxygen carrier prepared in Example 2 was evaluated for activity in a fixed bed reactor for methane chemical loop reforming reaction. The amount of oxygen carrier was 300 mg, and the particle size was 20-40 mesh. The fuel gas composition was 5% CH4 / Ar, the flow rate was 15 ml / min, the reaction temperature was 800°C, the reaction time was 15 min, and the reaction pressure was normal pressure.
[0079] Example 9
[0080] The oxygen carrier prepared in Example 2 was evaluated for activity in a fixed bed reactor for methane chemical loop reforming reaction. The amount of oxygen carrier was 300 mg, and the particle size was 20-40 mesh. The fuel gas composition was 5% H2O / Ar, the flow rate was 15 ml / min, the reaction temperature was 950°C, the reaction time was 15 min, and the reaction pressure was normal pressure.
[0081] Example 10
[0082] Pr 0.1 La 0.9 Preparation of FeO3 oxygen carrier
[0083] According to the molar ratio of 1:9:10, a certain mass of Pr(NO)3·6H2O, La(NO3)3·6H2O, and Fe(NO3)3·9H2O were weighed and dissolved in 60℃ deionized water. After continuous heating and stirring, after complete dissolution, a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) was weighed in another beaker and stirred to dissolve. At this time, the metal precursor solution with a concentration of 1.0 mol / L was poured into the citric acid solution. After the citric acid was fully dissolved, a small amount of isopropanol dispersion solution was added dropwise, and the specific amount was 0.9% of the total volume of the precursor solution. After that, the mixed solution was placed in a constant temperature water bath at 80℃ and stirred to fully evaporate the water in the solution. The remaining porous viscous colloid was dried at 120℃ for 600 minutes to obtain a yellow-brown brittle precursor. The precursor was fully ground and the sample was calcined in a muffle furnace, first heated to 300°C at a heating rate of 10°C per minute and retained for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 800°C at a heating rate of 10°C per minute and retained for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles at a pressure of 15MPa to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0084] Embodiment 11
[0085] Pr 0.2 La 0.8 Preparation of FeO3 oxygen carrier
[0086] The specific operation is the same as that of Example 10, except that the molar ratio of Pr(NO)3·6H2O to La(NO3)3 in the precursor solution is 2:8.
[0087] Example 12
[0088] Pr 0.4 La 0.6 Preparation of FeO3 oxygen carrier
[0089] The specific operation is the same as that of Example 10, except that the molar ratio of Pr(NO)3·6H2O to La(NO3)3 in the precursor solution is 4:6.
[0090] Embodiment 13
[0091] Pr 0.6 La 0.4 Preparation of FeO3 oxygen carrier
[0092] The specific operation is the same as that of Example 10, except that the molar ratio of Pr(NO)3·6H2O to La(NO3)3 in the precursor solution is 6:4.
[0093] Embodiment 14
[0094] Pr0.8 La 0.2 Preparation of FeO3 oxygen carrier
[0095] The specific operation is the same as that of Example 10, except that the molar ratio of Pr(NO)3·6H2O to La(NO3)3 in the precursor solution is 8:2.
[0096] Embodiment 15
[0097] Preparation of PrFeO3 oxygen carrier
[0098] The specific operation is the same as that of Example 10, except that the precursor solution contains only Pr(NO)3·6H2O and Fe(NO3)3, and the molar ratio of Pr(NO)3·6H2O to Fe(NO3)3 is 1:1.
[0099] Example 16
[0100] Pr 0.2 La 0.8 Fe 0.9 Co 0.1 Preparation of O3 oxygen carrier
[0101] According to the molar ratio of 2:8:9:1, a certain amount of Pr(NO)3·6H2O, La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O were weighed and dissolved in 60℃ deionized water, and continued to heat and stir. After complete dissolution, a certain amount of citric acid solid (citric acid: metal cation = 2.5:1) was weighed in another beaker and stirred to dissolve. At this time, the metal precursor solution with a concentration of 1.0 mol / L was poured into the citric acid solution. After the citric acid was fully dissolved, a small amount of isopropanol dispersion solution was added dropwise, and the specific amount was 1% of the total volume of the precursor solution. After that, the mixed solution was placed in a constant temperature water bath at 80℃ and stirred to fully evaporate the water in the solution. The remaining porous viscous colloid was dried at 120℃ for 600 minutes to obtain a yellow-brown brittle precursor. The precursor was fully ground and the sample was calcined in a muffle furnace, first heated to 400°C at a heating rate of 10°C per minute and retained for 120 minutes to fully remove organic impurities in the sample. Then the temperature was continuously raised to 1000°C at a heating rate of 10°C per minute and retained for 180 minutes. The obtained oxygen carrier powder was pressed into 20-40 mesh particles at a pressure of 15MPa to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
[0102] Embodiment 17
[0103] Pr 0.2 La 0.8 Fe 0.5 Co 0.5 Preparation of O3 oxygen carrier
[0104] The specific operation is the same as that of Example 16, except that the molar ratio of Pr(NO)3·6H2O, La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O in the precursor solution is 2:8:5:5.
[0105] Embodiment 18
[0106] Pr 0.2 La 0.8 Fe 0.3 Co 0.7 Preparation of O3 oxygen carrier
[0107] The specific operation is the same as that of Example 16, except that the molar ratio of Pr(NO)3·6H2O, La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O in the precursor solution is 2:8:3:7.
[0108] Embodiment 19
[0109] Pr 0.2 La 0.8 Fe 0.1 Co 0.9 Preparation of O3 oxygen carrier
[0110] The specific operation is the same as that of Example 16, except that the molar ratio of Pr(NO)3·6H2O, La(NO3)3·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O in the precursor solution is 2:8:1:9.
[0111] Embodiment 20
[0112] The oxygen carrier prepared in Examples 10-20 was evaluated for activity in a fixed bed reactor for methane chemical loop reforming reaction. The amount of oxygen carrier was 300 mg, and the particle size was 20-40 mesh. The fuel gas composition was 5% CH4 / Ar, the flow rate was 15 ml / min, the reaction temperature was 900°C, the reaction time was 20 min, and the reaction pressure was normal pressure.
[0113] The above are only some examples of the present invention, and do not limit the present invention in any form; any technician familiar with the field can use the above method to make many possible modifications, equivalent substitutions or improvements to the present invention without departing from the scope of the technical solution of the present invention. Therefore, any simple modification, equivalent substitution, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.
Claims
1. An oxygen carrier for producing synthesis gas by chemical loop reforming of methane, characterized in that: The oxygen carrier has a perovskite structure and the chemical formula is Pr x La 1-x Co y Fe 1-y O3, where 0 <x≤1,0≤y≤1。 2. The oxygen carrier for producing synthesis gas by chemical looping reforming of methane according to claim 1, characterized in that: x is 0.1, 0.2, 0.4, 0.6 or 0.8, and y is 0.1, 0.3, 0.5, 0.7 or 0.
9.
3. A method for preparing an oxygen carrier for producing synthesis gas through methane chemical loop reforming, characterized in that: The following steps are involved: Press Pr x La 1-x Fe y Co 1-y O3, dissolving the precursor of Pr, the precursor of La, the precursor of Co and the precursor of Fe in hot water to form a precursor solution; wherein, 0 <x≤1,0≤y≤1; Add a hot citric acid aqueous solution to a precursor solution, then add ethylene glycol or isopropanol, stir under heating conditions until it is in a gel state, dry, calcine, and shape to obtain an oxygen carrier for methane chemical chain reforming to produce synthesis gas.
4. The method for preparing an oxygen carrier for producing synthesis gas through methane chemical looping reforming according to claim 1, characterized in that: The precursor of Pr is at least one of Pr(NO3)3·6H2O, Pr(CH3COO)3·xH2O and Pr2(SO4)3·8H2O; the precursor of La is at least one of La(NO3)3·6H2O and La(CH3COO)3·xH2O; the precursor of Fe is at least one of FeCl3, Fe(NO3)3·9H2O and FeSO4; the precursor of Co is at least one of Co(NO3)2·6H2O, Co(CH3COO)2·4H2O.
5. The method for preparing an oxygen carrier for producing synthesis gas through methane chemical looping reforming according to claim 3, characterized in that: The total concentration of the Pr precursor, the La precursor, the Co precursor and the Fe precursor in the precursor solution is 0.9 to 1.5 mol / L.
6. The method for preparing an oxygen carrier for producing synthesis gas through methane chemical looping reforming according to claim 3, characterized in that: The amount of citric acid used is 1.5 to 2.5 times the total molar amount of Pr, La, Co and Fe ions.
7. The method for preparing an oxygen carrier for producing synthesis gas through methane chemical looping reforming according to claim 3, characterized in that: The amount of ethylene glycol or isopropanol used is 0.5-1.2% of the total volume of the precursor solution and the citric acid solution.
8. The method for preparing an oxygen carrier for producing synthesis gas through methane chemical looping reforming according to claim 3, characterized in that: The specific process of calcination is: first calcining at 300-500°C for 2-5h, and then calcining at 800-1000°C for 2-5h.
9. Use of the oxygen carrier according to any one of claims 1 or 2 in methane chemical loop reforming to produce synthesis gas, characterized in that: The oxygen carrier circulates between two interconnected fuel reactors and a regeneration reactor; wherein, in the fuel reactor, the oxygen carrier oxidizes methane at 700-1000° C. to produce synthesis gas; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 700-1000° C. in an oxidizing atmosphere; The fuel reactor contains a mixture of methane and inert gas.
10. The use according to claim 9, characterized in that: The oxidizing atmosphere is a mixture of any one of carbon dioxide, oxygen, water vapor and an inert gas, or the oxidizing atmosphere is a mixture of water vapor and carbon dioxide; The volume fraction of methane in the mixture of methane and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of carbon dioxide and inert gas, the volume fraction of carbon dioxide in the mixture of carbon dioxide and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of water vapor and inert gas, the volume fraction of water vapor in the mixture of water vapor and inert gas is 1% to 100%. When the oxidizing atmosphere is a mixture of oxygen and inert gas, the volume fraction of oxygen in the mixture of oxygen and inert gas is 1% to 100%.