Preparation methods of lithium iron phosphate materials, positive electrode plates and batteries
By adding antimony powder or bismuth powder to the lithium iron phosphate precursor, the thermal shrinkage property of the particles is utilized to make them shrink tightly, thus solving the problem of low compaction density of lithium iron phosphate materials and achieving improved material performance and simplified process.
Patent Information
- Application Number
- CN202310372742.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-04-10
AI Technical Summary
In the existing technology, lithium iron phosphate materials have low compaction density, resulting in low volumetric energy density, and existing methods to improve it are cumbersome and ineffective.
Antimony powder or bismuth powder is uniformly mixed into the lithium iron phosphate precursor. Its thermal shrinkage property is used to make the particles shrink tightly during the sintering process, thereby increasing the compaction density and avoiding increasing the particle size or reducing the carbon coating.
This method increases the compaction density of lithium iron phosphate materials to 2.7 g/cm3, simplifies the preparation process, and improves the material's performance.
Smart Images

Figure CN118771333B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium iron phosphate materials, specifically to a method for preparing lithium iron phosphate materials, a positive electrode sheet, and a battery. Background Technology
[0002] Compared to other lithium-ion battery cathode materials, lithium iron phosphate (LFP) batteries have advantages in overall performance indicators such as safety, cycle life, and production cost. Currently, LFP batteries are widely used in many fields, including electric vehicles, automobiles, ships, and energy storage, becoming one of the most promising power batteries at present. However, the low volumetric energy density limits the application of LFP cathode materials, and the key to increasing volumetric energy density lies in improving compaction density.
[0003] In existing technologies, methods to improve the compaction density of lithium iron phosphate materials include increasing the particle size of the lithium iron phosphate material and reducing the amount of carbon coating on the surface of the lithium iron phosphate. However, increasing the particle size will reduce its capacity and deteriorate its rate performance; reducing the amount of carbon coating on the particle surface will cause the material to easily agglomerate. Moreover, the above methods are cumbersome. Summary of the Invention
[0004] In view of this, this application provides a preparation method that can improve the compaction density of lithium iron phosphate materials, and the method is simple.
[0005] This application provides a method for preparing lithium iron phosphate material, comprising the following steps:
[0006] Metal powder, including at least one of antimony powder or bismuth powder, is added to a lithium iron phosphate precursor and mixed evenly to obtain a sintering precursor.
[0007] Sintering the sintering precursor;
[0008] The sintered precursor was naturally cooled to room temperature and crushed to obtain powdered lithium iron phosphate material.
[0009] Optionally, the sintering includes the following steps:
[0010] Sintering is carried out at 250-650℃ for 2-4 hours, followed by heating to 750-800℃ for 8-12 hours at a heating rate of 2-5℃ / min. The sintering is carried out under vacuum or in a protective atmosphere with a flow rate of 10-40L / min and an oxygen content of less than 50ppm.
[0011] Optionally, the mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor.
[0012] Optionally, the particle size of the lithium iron phosphate precursor is 0.3-2 μm.
[0013] Optionally, the particle size of the metal powder is less than 20 μm.
[0014] Optionally, the lithium iron phosphate precursor includes a lithium source, an iron source, and a carbon source, wherein the molar ratio of the lithium source to the iron source is 0.96-1.04, the mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source, and the iron source or the lithium source includes phosphate.
[0015] Optionally, the preparation of the lithium iron phosphate precursor includes:
[0016] The lithium source, the iron source, and the carbon source are mixed in stoichiometric ratios, and deionized water is added to obtain a mixture.
[0017] The mixture is then subjected to wet ball milling and dried.
[0018] This application also provides a positive electrode sheet, including a positive electrode material, wherein the positive electrode material includes lithium iron phosphate material obtained by the preparation method of the lithium iron phosphate material described above.
[0019] This application also provides a battery, the battery including the aforementioned positive electrode plate.
[0020] Compared to existing technologies, this application uniformly mixes antimony or bismuth powder into the lithium iron phosphate precursor, ensuring that the antimony or bismuth powder is evenly dispersed among the particles of the lithium iron phosphate precursor. Due to the thermal shrinkage property of antimony or bismuth powder, its crystal structure and atomic arrangement change with increasing temperature, resulting in a denser atomic arrangement and volume reduction. During the sintering process to form lithium iron phosphate, the antimony or bismuth powder causes the lithium iron phosphate precursor particles to shrink tightly together, reducing the interparticle spacing and thus increasing the compaction density of the lithium iron phosphate material to at least 2.7 g / cm³. 3 Furthermore, this application only shrinks the lithium iron phosphate precursor, eliminating the need to increase the size of lithium iron phosphate particles or reduce the carbon coating on the particle surface, thus simplifying the lithium iron phosphate preparation process. Attached Figure Description
[0021] Figure 1 The flowchart for preparing lithium iron phosphate provided in this application;
[0022] Figure 2 This is a SEM image of the lithium iron phosphate material provided in Embodiment 1 of this application. Detailed Implementation
[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0025] The following detailed description of some embodiments of the present invention is provided in conjunction with the accompanying drawings. Unless otherwise specified, the following embodiments and features can be combined with each other.
[0026] Reference Figure 1 This application provides a method for preparing lithium iron phosphate, the method comprising the following steps:
[0027] Step S101: Add metal powder, including at least one of antimony powder or bismuth powder, to the lithium iron phosphate precursor particles, and mix thoroughly to obtain a sintering precursor. A high-speed mixer can be used to obtain the sintering precursor.
[0028] In some embodiments, the lithium iron phosphate precursor particles include a lithium source, an iron source, and a carbon source, wherein the molar ratio of the lithium source to the iron source is 0.96-1.04, and the mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source. The lithium source or the iron source includes phosphate. The lithium source may include at least one of lithium carbonate, lithium hydroxide, lithium chloride, lithium sulfate, lithium acetate, lithium phosphate, and lithium nitrate. The iron source may include at least one of iron phosphate, iron nitrate, and ferrous sulfate. The carbon source may include at least one of glucose, sucrose, polyethylene glycol, and lactose.
[0029] In some embodiments, the preparation of the lithium iron phosphate precursor may include the following steps:
[0030] The lithium source, iron source, and carbon source are mixed according to a stoichiometric ratio, and deionized water is added to obtain a mixture. Optionally, the mass of the deionized water is 30-60% of the total mass of the lithium source, iron source, and carbon source. The selection of this deionized water ratio ensures uniform mixing of the lithium source, iron source, and carbon source, while also reducing energy consumption in subsequent steps.
[0031] The mixture is wet-ball-milled and dried. The ball-milled mixture can be dried by spray granulation to obtain the lithium iron phosphate precursor. Optionally, the particle size of the lithium iron phosphate precursor can be 0.3-2 μm.
[0032] In another embodiment, the particle size of the lithium iron phosphate precursor may be less than 0.3 μm or greater than 2 μm.
[0033] In another embodiment, the lithium iron phosphate precursor can be obtained by dry grinding.
[0034] In some embodiments, the mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor. The particle size of the metal powder is less than 20 μm.
[0035] In another embodiment, the mass ratio of the metal powder to the lithium iron phosphate precursor particles may be less than 0.03 or greater than 0.1.
[0036] Step S102: Sinter the sintering precursor. The sintering includes the following steps:
[0037] Sintering is carried out at 250-650℃ for 2-4 hours, followed by sintering at 750-800℃ for 8-12 hours. The heating rate is 2-5℃ / min. The sintering is performed under vacuum or in a protective atmosphere with a flow rate of 10-40 L / min, wherein the oxygen content in the protective atmosphere is below 50 ppm. The protective gas includes, but is not limited to, nitrogen.
[0038] During the sintering process, the iron source, the lithium source, and the carbon source react to generate lithium iron phosphate.
[0039] Step S103: The sintered precursor is naturally cooled to room temperature and then crushed to obtain powdered lithium iron phosphate material. The sintered precursor can be crushed by grinding or air jet milling.
[0040] This application uniformly mixes antimony powder or bismuth powder into a lithium iron phosphate precursor, ensuring that the antimony or bismuth powder is evenly dispersed among the particles of the lithium iron phosphate precursor. Due to the thermal shrinkage property of antimony or bismuth powder, its crystal structure and atomic arrangement change with increasing temperature, resulting in a denser atomic arrangement and volume reduction. During the sintering process to form lithium iron phosphate, the antimony or bismuth powder causes the lithium iron phosphate precursor particles to shrink tightly together, reducing the inter-particle spacing and thus increasing the compaction density of the lithium iron phosphate material to at least 2.7 g / cm³. Furthermore, this application only shrinks the lithium iron phosphate precursor, eliminating the need to further increase the size of the lithium iron phosphate particles or reduce the carbon coating on the particle surface, thus simplifying the lithium iron phosphate preparation process.
[0041] This application also provides a positive electrode sheet, including a positive electrode material, wherein the positive electrode material includes lithium iron phosphate material obtained by the preparation method of the lithium iron phosphate material described above.
[0042] Specifically, in some embodiments, the lithium iron phosphate material can be prepared into a positive electrode sheet through the following steps:
[0043] A binder slurry is prepared, and a conductive additive is added to the binder slurry to prepare a first slurry. Then, lithium iron phosphate is added to the first slurry to prepare a second slurry. The second slurry is coated on aluminum foil and then baked to obtain a positive electrode sheet.
[0044] This application also provides a battery (not shown), which includes the positive electrode. Specifically, the battery may further include a negative electrode and a separator.
[0045] Specifically:
[0046] Example 1:
[0047] 36.64 g of lithium carbonate, 150.82 g of iron phosphate, 11.31 g of glucose, and 281.20 g of deionized water were weighed and added together to a mixing tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was then dried by spray drying to obtain granular lithium iron phosphate precursor.
[0048] Antimony powder is added to the lithium iron phosphate precursor. The mass of the antimony powder is 3% of the mass of the lithium iron phosphate precursor, and the particle size of the antimony powder is 15 μm. The lithium iron phosphate precursor and antimony powder are mixed evenly by a high-speed mixer to obtain a sintering precursor.
[0049] The sintering precursor was placed in a box furnace for sintering under a nitrogen atmosphere with a flow rate of 25 L / min and an oxygen content of less than 50 ppm. The sintering was first performed at 630°C for 2 hours, followed by a further heating to 780°C at a rate of 5°C / min and sintering for another 11 hours.
[0050] The sintered precursor was naturally cooled to room temperature and then subjected to airflow crushing to obtain powdered lithium iron phosphate product. The SEM image of the lithium iron phosphate product is shown below. Figure 2 As shown.
[0051] Example 2:
[0052] Unlike Example 1, the antimony powder is 5% of the mass of the lithium iron phosphate precursor, the particle size of the antimony powder is 10 μm, and the sintering precursor is first sintered at 640°C for 3 hours, and then heated to 790°C for 12 hours.
[0053] Example 3:
[0054] Unlike Example 1, the antimony powder is 7% of the mass of the lithium iron phosphate precursor, the particle size of the antimony powder is 8 μm, and the sintering precursor is first sintered at 650°C for 4 hours, and then heated to 800°C for 12 hours.
[0055] Example 4:
[0056] 36.64 g of lithium carbonate, 150.82 g of iron phosphate, 11.31 g of glucose, and 281.20 g of deionized water were weighed and added together to a mixing tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was then dried by spray drying to obtain granular lithium iron phosphate precursor.
[0057] Bismuth powder is added to the lithium iron phosphate precursor, wherein the mass of the bismuth powder is 3% of the lithium iron phosphate precursor and the particle size of the bismuth powder is 15 μm. The lithium iron phosphate precursor and bismuth powder are mixed evenly using a high-speed mixer to obtain a sintering precursor.
[0058] The sintering precursor was placed in a box furnace for sintering. The sintering was carried out in a nitrogen atmosphere with a flow rate of 25 L / min and an oxygen content of less than 50 ppm. The sintering was first carried out at 270 °C for 2 hours, and then the temperature was increased to 780 °C at a heating rate of 5 °C / min and sintered for another 11 hours.
[0059] The sintered precursor was naturally cooled to room temperature and then subjected to airflow crushing to obtain powdered lithium iron phosphate product.
[0060] Example 5:
[0061] Unlike Example 4, the bismuth powder accounts for 5% of the mass of the lithium iron phosphate precursor, and the particle size of the bismuth powder is 10 μm. The sintering precursor is first sintered at 280°C for 4 hours, and then heated to 790°C for 12 hours.
[0062] Example 6:
[0063] Unlike Example 4, the bismuth powder accounts for 7% of the mass of the lithium iron phosphate precursor, and the particle size of the bismuth powder is 8 μm. The sintering precursor is first sintered at 290°C for 4 hours, and then heated to 800°C for 12 hours.
[0064] Example 7:
[0065] Unlike Example 1, antimony powder and bismuth powder were added to the lithium iron phosphate precursor. The antimony powder had a particle size of 10 μm. The bismuth powder accounted for 3% of the mass of the lithium iron phosphate precursor, and its particle size was 8 μm. The lithium iron phosphate precursor, antimony powder, and bismuth powder were mixed uniformly using a high-speed mixer to obtain a sintering precursor.
[0066] Comparative Example 1:
[0067] 36.64 g of lithium carbonate, 150.82 g of iron phosphate, 11.31 g of glucose, and 281.20 g of deionized water were weighed and added together to a mixing tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was then dried by spray drying to obtain granular lithium iron phosphate precursor.
[0068] The sintering precursor was sintered in a box furnace under a nitrogen atmosphere of 25 L / min, with the oxygen content controlled below 50 ppm. The sintering was first carried out at a low temperature of 270°C for 2 h, and then the temperature was increased to 780°C for 12 h. The heating rate was 5°C / min.
[0069] The sintered precursor is cooled to room temperature. Then, the cooled sintered precursor is subjected to airflow crushing to obtain powdered lithium iron phosphate product.
[0070] This application uses the following method to test the compaction density of powdered lithium iron phosphate.
[0071]
[0072]
[0073] Lithium iron phosphate was used to prepare electrodes. The electrodes, negative electrode shell, lithium metal sheet, separator, gasket, spring sheet, positive electrode shell, and electrolyte were then assembled into a button cell. Charge-discharge tests were performed on the battery. The specific battery testing method is as follows:
[0074]
[0075]
[0076] The test results of the compaction density of the lithium iron phosphate powder obtained in Examples 1-7 and Comparative Example 1 are as follows.
[0077]
[0078] The test results above show that the compaction density of the lithium iron phosphate in Comparative Example 1 without the addition of antimony powder or bismuth powder is 2.4 g / cm³. 3Approximately. In Examples 1-7, when different proportions of antimony powder or bismuth powder are added to the lithium iron phosphate precursor, the compaction density of the lithium iron phosphate can be increased to at least 2.7 g / cm³. 3 .
[0079] The above description is merely a preferred embodiment of this application and does not limit the patent scope of this application. Any equivalent structural transformations made based on the concept of this application and the contents of the specification and drawings of this application, or direct / indirect applications in other related technical fields, are included within the patent protection scope of this application.
Claims
1. A method for preparing lithium iron phosphate material, characterized in that, Includes the following steps: Metal powder, including at least one of antimony powder or bismuth powder, is added to a lithium iron phosphate precursor and mixed evenly to obtain a sintering precursor. The mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor. The sintering of the sintering precursor includes the following steps: sintering at 250-650℃ for 2-4 hours, followed by heating to 750-800℃ for 8-12 hours, with a heating rate of 2-5℃ / min. The sintering is carried out under vacuum conditions or in a protective atmosphere with a flow rate of 10-40L / min, wherein the oxygen content in the protective atmosphere is below 50ppm. The sintered precursor was naturally cooled to room temperature and crushed to obtain powdered lithium iron phosphate material.
2. The method for preparing lithium iron phosphate material as described in claim 1, characterized in that, The particle size of the lithium iron phosphate precursor is 0.3-2 μm.
3. The method for preparing lithium iron phosphate material as described in claim 2, characterized in that, The particle size of the metal powder is less than 20 μm.
4. The method for preparing lithium iron phosphate material as described in claim 1, characterized in that, The lithium iron phosphate precursor includes a lithium source, an iron source, and a carbon source. The molar ratio of the lithium source to the iron source is 0.96-1.
04. The mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source. The iron source or the lithium source includes phosphate.
5. The method for preparing lithium iron phosphate material as described in claim 4, characterized in that, The preparation of the lithium iron phosphate precursor includes: The lithium source, the iron source, and the carbon source are mixed in stoichiometric ratios, and deionized water is added to obtain a mixture. The mixture is then subjected to wet ball milling and dried.
6. A positive electrode sheet, comprising a positive electrode material, characterized in that, The cathode material includes lithium iron phosphate material prepared by the method described in any one of claims 1 to 5.
7. A battery, characterized in that, The battery includes the positive electrode as described in claim 6.
Citation Information
Patent Citations
Method for enhancing conductivity of lithium iron phosphate material
CN102403502A