Method for preparing hollow calcium silicate board by using high-silicon iron tailings and quicklime
Patent Information
- Application Number
- CN202410817716.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2026-11-03
- Estimated Expiration
- 2044-06-24
AI Technical Summary
High-silicon iron tailings, when used to prepare calcium silicate boards, cause deformation and mold collapse due to the iron content, making them unsuitable for direct use in building materials. Furthermore, traditional quartz sand is too expensive to meet the needs of industrial production.
Hollow calcium silicate boards are prepared by using high-silicon iron tailings and quicklime as the main raw materials, with the addition of sand and gravel aggregates, cement, fiber and chemical raw materials, through extrusion molding and high-temperature autoclaving. The proportion of each raw material and process parameters are controlled to solve the problems of plasticity and strength.
This paper presents a method for the resource utilization of high-silicon iron tailings to produce high-quality and inexpensive hollow calcium silicate boards that meet the performance requirements of prefabricated buildings, reduce engineering costs, and improve compressive strength and impact resistance.
Smart Images

Figure CN118771840B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing hollow calcium silicate boards using high-silicon iron tailings and quicklime, belonging to the field of industrial solid waste resource utilization technology. Background Technology
[0002] Iron tailings are a large amount of industrial solid waste discharged during the iron ore washing process. Iron tailings from Tangshan in Hebei Province, Anshan in Liaoning Province, and Lueyang in Shaanxi Province have a silicon content of over 80%, and are also known as high-silicon iron tailings. The reserves of high-silicon iron tailings are enormous; the Sijiaying Iron Mine in Tangshan, Hebei Province alone discharges over 2 million tons of high-silicon iron tailings annually. Large quantities of high-silicon iron tailings are piled up in the mountains, causing serious pollution to the surrounding air and water environments and occupying a large amount of land. Researching comprehensive utilization technologies for high-silicon iron tailings can effectively alleviate pollution problems and save money for enterprises.
[0003] Prefabricated construction is a new construction industry promoted by national macro policies in recent years, with a huge market size. Prefabricated buildings no longer use masonry materials for interior walls, opting instead for panel-type building materials. Currently, the main panel-type building materials include foamed ceramic panels and autoclaved aerated concrete (AAC). However, mainstream interior wall panel materials on the market are expensive and suffer from problems such as cracking at the joints, difficulty in nailing, and inability to achieve integrated construction of the decorative surface layer. Calcium silicate board is a new type of board made from loose short fibers such as inorganic mineral fibers as reinforcement, with siliceous and calcareous materials as the main materials, through a series of processes including pulping and molding. The siliceous raw material is generally quartz sand, but ordinary quartz sand has a coarse particle size and poor properties, and the strength of the reacted product cannot meet the performance requirements of building materials. Only ultrafine quartz sand can be used, but ultrafine quartz sand is expensive and cannot meet the cost control requirements of industrial production. High-silicon iron tailings are ultrafine industrial solid waste produced during iron ore beneficiation. They are characterized by high silicon content and fine particle size. When high-silicon iron tailings are used to replace the siliceous natural quartz sand added in the traditional calcium silicate board production process, the iron introduced by the tailings disrupts the hydration reaction, leading to deformation and mold collapse during autoclaving. This makes high-silicon iron tailings unsuitable for direct use in calcium silicate board production. Therefore, effectively addressing the deformation and mold collapse problems encountered when using high-silicon iron tailings in calcium silicate board preparation is a pressing technical issue.
[0004] This invention uses high-silicon iron tailings as the main raw material and provides a high-quality and inexpensive board material for prefabricated buildings, solving two problems that urgently need to be addressed in the industry. Summary of the Invention
[0005] (a) Technical problems to be solved
[0006] To address the aforementioned problems in the prior art, this invention provides a method for preparing hollow calcium silicate plates using high-silicon iron tailings and quicklime.
[0007] (II) Technical Solution
[0008] To achieve the above objectives, the main technical solutions adopted by the present invention include:
[0009] A method for preparing hollow calcium silicate boards using high-silicon iron tailings and quicklime includes the following steps:
[0010] S1. Using high-silicon iron tailings and quicklime as the main raw materials, sand and gravel aggregates, cement, fiber and chemical raw materials are added, and water is added and stirred and mixed. The chemical raw materials include reinforcing agents, degumming agents and plasticizers.
[0011] S2. The mixed mud is extruded into shape;
[0012] S3. After molding, the green body is cured by high-temperature steam pressing to prepare hollow calcium silicate board.
[0013] In the method described above, preferably, in step S1, by weight, the high-silicon iron tailings are 20-30 parts, the quicklime is 20-30 parts, the sand and gravel aggregate is 10-20 parts, the cement is 10-20 parts, the fiber is 10-20 parts, the reinforcing agent is nickel chloride 0.5-1 parts, the degumming agent is calcium stearate 1-5 parts, and the plasticizer is sodium carboxymethyl cellulose 1-5 parts.
[0014] In the method described above, preferably, the main component of the ferrosilicon tailings is silicon dioxide, and the silicon dioxide content is greater than 80%.
[0015] In the method described above, preferably, the main component of the quicklime is calcium oxide, and the calcium oxide content is 70-98%.
[0016] In the method described above, preferably, the fiber is one or a combination of several of the following: aluminum silicate fiber, glass wool, rock wool, and polypropylene fiber.
[0017] In the method described above, preferably, in step S1, the amount of water used is 15-19% of the total weight of the raw materials; the stirring and mixing are carried out using a planetary mixer, the mixing time is 10-30 minutes, and the weight deviation of the sieved sand and gravel aggregate is ≤10%.
[0018] In the method described above, preferably, in step S2, the extrusion molding is performed using an extruder with a vacuum degree of 10-100 Pa, an extrusion pressure of 1-5 MPa, and a discharge speed of 10-20 m / min.
[0019] In the method described above, preferably, in step S3, the high-temperature autoclaving is carried out in an autoclaving kiln, the curing temperature is 195-240℃, the curing time is 2-4 hours, and the curing pressure is 1.5-2 MPa.
[0020] Hollow calcium silicate board prepared by the method described above.
[0021] (III) Beneficial Effects
[0022] The beneficial effects of this invention are:
[0023] The present invention provides a method for preparing hollow calcium silicate boards using high-silicon iron tailings and quicklime. First, high-silicon iron tailings and quicklime are used as the main raw materials, and sand and gravel aggregates, cement, fiber and chemical raw materials are added, and water is added and stirred and mixed evenly. Then, the mixed mud is formed by extrusion. The formed green body is then cured by high-temperature autoclaving to prepare hollow calcium silicate boards.
[0024] The method provided by this invention offers a resource utilization approach for high-silicon iron tailings, which are difficult to utilize, and can effectively alleviate the problem of high environmental protection expenditure pressure on mining enterprises. At the same time, it provides a revolutionary high-quality and inexpensive wall material for prefabricated buildings, which is of great significance for solving the problem of slow development of the prefabricated building industry due to material constraints.
[0025] On a technical level, this invention applies extrusion molding technology to the calcium silicate board industry, upgrading traditional flat calcium silicate products into hollow, three-dimensional boards. The board thickness, strength, and sound insulation performance can be flexibly designed and adjusted. The hollow portion of the board meets the installation requirements of pipework in prefabricated building walls, providing a revolutionary, high-quality, and inexpensive wall material for the prefabricated building industry. This facilitates the transformation of calcium silicate boards from decorative materials engineering to wall materials. The thickness of the hollow calcium silicate strips is adjustable from 6-22cm, and the density is 400-1200kg / m³. 3 It is adjustable, with a compressive strength of over 10MPa (while the national standard is 3.5MPa), and an impact resistance of over 20 times (while the national standard is 5 times), making it a superior product. Attached Figure Description
[0026] Figure 1 This is a flowchart illustrating the method of the present invention. Detailed Implementation
[0027] The principle of this invention is based on the hydrothermal synthesis technology of calcium silicate materials. Research has shown that using nickel chloride as a reinforcing agent promotes the hydrothermal reaction between the quartz phase in high-silicon iron tailings and quicklime, resulting in hollow calcium silicate strips with hard calcium silicate and tobermorite as the main crystalline phases. The clay components other than the quartz phase in the high-silicon iron tailings, along with the plasticizer sodium carboxymethyl cellulose, work together to regulate the plasticity of the clay, solving the problem of excessive foundation pressure caused by poor plasticity. The addition of calcium stearate, a degumming agent, further reduces the water content of the clay under the same plasticity conditions. Simultaneously, the addition of rationally graded sand and gravel aggregates solves the industry-wide technical problem of green body deformation or mold collapse during autoclaving due to low green strength.
[0028] This invention, through extensive experimental research, has discovered that the main components of high-silicon iron tailings are quartz-phase silicate components and a small amount of clay components. The quartz-phase silicate components provide siliceous raw materials for the hydrothermal synthesis reaction of calcium silicate materials, while the clay components improve the plasticity of the clay. When the silica content is greater than 80%, the other components of the high-silicon iron tailings are relatively stable, with fewer components harmful to the hydration reaction. If the silica content is low, the reaction is incomplete, introducing too many impurities, which easily leads to insufficient strength of the slabs and failure to meet standard requirements. Therefore, it is preferable that the silica content, the main component, is greater than 80%. In this invention, if the amount of high-silicon iron tailings added is too small, the hydrothermal synthesis reaction of calcium silicate will be incomplete, resulting in a significant reduction in material strength. If the amount of high-silicon iron tailings added is too large, the introduced clay raw materials will increase, leading to excessive plasticity and enhanced water retention in the clay, resulting in reduced green strength. The material is prone to mold collapse during autoclaving, reducing the yield. Therefore, the high-silicon iron tailings are preferably 20-30% of the total weight of the raw materials.
[0029] Quicklime's main components are calcium oxide and a small amount of shale. Extensive experimental research has shown that quicklime with a calcium oxide content greater than 80% can be used to prepare calcium silicate boards. If the calcium oxide content is too low, the hollow board strength will be too low, failing to meet standard requirements, and therefore it cannot be used to prepare calcium silicate boards. Therefore, a calcium oxide content greater than 80% in quicklime is preferred. Quicklime provides calcium for the hydrothermal synthesis reaction of calcium silicate. According to the hydrothermal synthesis reaction equation SiO2 + CaO = CaSiO3, the theoretical molar ratio should be 1:1. If the reaction is complete, the mass ratio should be 60:56. However, the silica introduced from high-silicon iron tailings is a quartz component, which is relatively hard. The actual reaction process is not as complete as that of quicklime. In production, for ease of calculation, a mass ratio of 1:1 is used, meaning the weight ratio of calcium to silica is 1:1. Therefore, quicklime is preferably 20-30% of the total weight of the raw materials.
[0030] Experimental studies have shown that adding appropriate sand and gravel aggregates can reduce the moisture content of the clay while maintaining its plasticity. The principle is that the space occupied by the aggregates in the green body does not require water wetting. Insufficient sand and gravel aggregates cannot effectively reduce the moisture content of the green body, thus failing to prioritize increasing its strength. In this invention, excessive sand and gravel aggregates reduce the proportion of siliceous and calcareous components, leading to incomplete hydrothermal synthesis reactions and a significant decrease in the strength of the material after autoclaving. Therefore, the sand and gravel aggregates are preferably 10-20% of the total weight of the raw materials.
[0031] Cement provides initial strength to the green body. Before the green body enters the high-temperature curing kiln after extrusion molding, the hydrothermal synthesis reaction of silicon and calcium has not yet occurred; the strength of the green body mainly comes from the extrusion molding pressure and the plasticity of the clay material. During this process, the hydration reaction of cement provides strength compensation for the green body. If the amount of cement added is too low, the provided strength will be insufficient, easily leading to mold collapse and green body deformation. If the amount of cement added is too high, it will increase material costs. Therefore, the preferred amount of cement added is 10-20% of the total weight of the raw materials.
[0032] Fiber materials can improve the flexural strength of the hollow structure of calcium silicate boards and suppress the downward bending deformation of the unsupported upper surface layer of the green hole structure. If the amount of fiber added is too small, the strength provided will be insufficient. If the amount added is too large, it will increase the material cost. Therefore, the fiber is preferably one of aluminosilicate fiber, glass wool, rock wool, or polypropylene fiber. Preferably, the amount of fiber added is 10-20%.
[0033] Chemical raw materials serve as fine-tuning components for the properties of the clay and the hydrothermal synthesis reaction. Nickel chloride acts as a reinforcing agent, promoting the hydrothermal reaction between the quartz phase in high-silicon iron tailings and quicklime to obtain hollow calcium silicate strips with hard silicate and tobermorite as the main crystalline phases. The clay components other than the quartz phase in the high-silicon iron tailings, along with the plasticizer sodium carboxymethyl cellulose, work together to adjust the plasticity of the clay, solving the problem of excessive foundation pressure caused by poor plasticity. The addition of the desiccant calcium stearate further reduces the water content of the clay under the same plasticity conditions. Calcium stearate is preferred as the desiccant due to its low price; water glass or sodium hexametaphosphate can also be used. Insufficient chemical raw materials will not achieve the desired effect, while excessive addition will increase material costs. Therefore, the preferred chemical raw materials are: reinforcing agent nickel chloride 0.5–1%, desiccant calcium stearate 1–5%, and plasticizer sodium carboxymethyl cellulose 1–5%.
[0034] The purpose of controlling the amount of water is to adjust the plasticity of the batch material and ensure that the pressure of the extruder is not too high during the extrusion process. If there is too little water, the extrusion pressure will be too high and the sheet material will not be extruded smoothly. If there is too much water, the moisture content of the green body will be too high, the strength of the green body will be low, and the die will collapse. Therefore, the preferred amount of water is 15 to 19% of the total weight of the raw materials.
[0035] In controlling the mixing and homogenization process parameters, various methods were tried, including ball mills, conical mixers, and V-type mixers. Research data shows that planetary mixers are more efficient and convenient. Too short a mixing time will not thoroughly mix the raw materials, while too long a mixing time will increase the energy consumption of the equipment. The preferred mixing time is 10–30 minutes. Using the weight deviation of the sieve residue as a basis for testing the uniformity of the mixture is convenient. A deviation higher than 10% can easily lead to incomplete hydrothermal synthesis of silicon and calcium, reducing the material's physical properties. Therefore, the preferred weight deviation of the sieve residue should be ≤10%. The weight deviation of the sieve residue is determined by taking 500g of the mixture five times, sieving it through a 60-mesh sieve. If the maximum and minimum weight deviation of the residue is less than or equal to 10%, it is considered homogenized.
[0036] The extrusion molding process is a key step in the preparation of hollow calcium silicate sheets in this invention. Vacuuming the clay material reduces the air bubble content in the green body after molding, which is beneficial to improving the strength of the green body. If the vacuum is too low, the residual gas content will not meet the requirements; if the vacuum is too high, a more expensive vacuum unit will be required. Therefore, the vacuum level is preferably 10-100 Pa. Extrusion pressure is the main control parameter for green body strength. Low extrusion pressure results in low green body strength and easy die collapse and deformation. Excessive extrusion pressure can easily lead to excessively high clay temperature, premature hydration, and reduced extrusion speed, resulting in reduced production efficiency. Therefore, the extrusion pressure is preferably 1-5 MPa. The discharge speed is related to the plasticity of the clay material, the extrusion pressure, and the die interface design. If the extrusion speed is too fast, it will lead to insufficient clay supply and cracks at the edges of the green body. If the extrusion speed is too slow, it will reduce production efficiency. Therefore, the preferred discharge speed is 10-20 m / min.
[0037] Autoclaving is a crucial stage in the final strength development of hollow calcium silicate boards, and the most mature equipment in China is the autoclaving kiln. Based on the calculated Kipling free energy of the calcium silicate hydrothermal synthesis reaction and extensive experimental data, low reaction temperatures inhibit the reaction process, while excessively high temperatures lead to increased costs. Insufficient curing time results in insufficient green strength, making the green body prone to collapse and deformation; prolonged curing also increases energy consumption and reduces production efficiency. Insufficient curing pressure leads to incomplete hydrothermal synthesis, reducing product strength; excessive curing pressure increases equipment investment and operating costs. Therefore, the optimal autoclaving temperature is 195–240℃, curing time is 2–4 hours, and pressure is 1.5–2 MPa.
[0038] The comprehensive cost of building a wall using the calcium silicate wall panel obtained by this invention is 120-150 yuan / square meter, while the cost of traditional masonry wall construction is 170-200 yuan / square meter, and the comprehensive cost of autoclaved aerated concrete panels commonly used in prefabricated buildings is 200-230 yuan / square meter. It can be seen that the preparation cost of this invention is low and it has high economic development and utilization value.
[0039] Specifically: A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime, the process diagram of which is shown below. Figure 1 As shown, it includes the following steps:
[0040] S1. Using high-silicon iron tailings and quicklime as the main raw materials, sand and gravel aggregates, cement, fiber, and chemical raw materials are added, and water is added and stirred and mixed evenly. The chemical raw materials include reinforcing agents, degumming agents, and plasticizers. Specifically, by weight, the high-silicon iron tailings comprise 20-30 parts, the quicklime 20-30 parts, the sand and gravel aggregates 10-20 parts, the cement 10-20 parts, the fiber 10-20 parts, the reinforcing agent is nickel chloride 0.5-1 part, the degumming agent is calcium stearate 1-5 parts, and the plasticizer is sodium carboxymethyl cellulose 1-5 parts. Further, the main component of the ferrosilicon tailings is silicon dioxide, with a silicon dioxide content greater than 80%; the main component of the quicklime is calcium oxide, with a calcium oxide content of 70-98%.
[0041] S2. The mixed mud is shaped by extrusion. Specifically, an extruder can be used. The vacuum degree of the extruder is 10-100 Pa, the extrusion pressure is 1-5 MPa, and the discharge speed is 10-20 m / min. The green body after extrusion has different channels along its length. The distribution of these hollow channels can be controlled by the holes in the die.
[0042] S3. The formed green body is subjected to high-temperature autoclaving to prepare hollow calcium silicate strips. The high-temperature autoclaving is carried out in an autoclaving kiln, the curing temperature is 195-240℃, the curing time is 2-4h, and the curing pressure is 1.5-2MPa.
[0043] The present invention provides the following advantages for manufacturing hollow calcium silicate boards: First, it solves the problem of heavy wall panels; the hollow design reduces the weight by three-quarters, significantly lowering installation costs. Second, the hollow design improves thermal insulation, sound insulation, and fire resistance, a major advantage compared to traditional wall panels. Third, the hollow design saves materials, significantly reducing material costs per square meter. Fourth, the hollow design allows for nailing. Therefore, the resulting hollow calcium silicate panels are inexpensive, high-strength, and can be nailed, cut, and processed. They can also be directly covered or sprayed with decorative coatings, completing wall construction and finishing in one step, greatly reducing project costs.
[0044] To better explain and facilitate understanding of the present invention, specific embodiments are described in detail below. Unless otherwise specified, all percentages (%) in the following examples are by weight. The cement used in the examples is ordinary silicate 425 cement. The chemical composition of the high-silicon iron tailings is: SiO2 82.6%, MgO 2.03%, TFe 1.34%, Al2O3 4.16%, CaO 6.16%, and other components 3.71%. The main chemical composition of the quicklime is: SiO2 2.15%, CaO 84.13%, Fe2O3 2.32%, Al2O3 4.66%, Na2O 3.4%, and other components 5.49%.
[0045] Example 1
[0046] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0047] S1. Prepare the following raw materials by weight: 30 parts high-silicon iron tailings, 30 parts quicklime, 10 parts sand and gravel aggregate, 10 parts cement, 10 parts polypropylene fiber, 1 part nickel chloride, 4 parts calcium stearate, and 5 parts sodium carboxymethyl cellulose.
[0048] A planetary mixer was used, and water was added at 15% of the total weight of the raw materials. The mixture was stirred and mixed for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.1%.
[0049] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 45Pa, the extrusion pressure is 3.5Mpa, and the discharge speed is 12.1m / min.
[0050] S3. After molding, the green body is placed in a high-temperature autoclave for curing at 200℃ for 2 hours and 2MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0051] Example 2
[0052] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0053] S1. Prepare the following raw materials by weight: 30 parts high-silicon iron tailings, 30 parts quicklime, 10 parts sand and gravel aggregate, 10 parts cement, 10 parts polypropylene fiber, 1 part nickel chloride, 4 parts calcium stearate, and 5 parts sodium carboxymethyl cellulose.
[0054] A planetary mixer was used to add water at 15% of the total weight of the raw materials, and the mixture was stirred and mixed for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.6%.
[0055] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 15Pa, the extrusion pressure is 5Mpa, and the discharge speed is 9.5m / min.
[0056] S3. After molding, the green body is placed in a high-temperature autoclave for curing at 220°C for 4 hours and 2MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0057] Example 3
[0058] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0059] S1. Add 10 parts of sand and gravel aggregate, 10 parts of cement, 10 parts of polypropylene fiber, 1 part of nickel chloride, 4 parts of calcium stearate, and 5 parts of sodium carboxymethyl cellulose to 30 parts of high silicon iron tailings and 30 parts of quicklime by weight.
[0060] A planetary mixer was used to add water at 19% of the total weight of the raw materials and mix them for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.4%.
[0061] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 90Pa, the extrusion pressure is 1.5Mpa, and the discharge speed is 18.2m / min.
[0062] S3. The formed green body is placed in a high-temperature autoclave for curing at 185°C for 1.2 hours and 1.2 MPa. After autoclaving, hollow calcium silicate strip material is obtained. Example 4
[0063] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0064] S1. Take 20 parts by weight of high-silicon iron tailings, 20 parts of quicklime, 20 parts of sand and gravel aggregate, 15 parts of cement, 15 parts of polypropylene fiber, 1 part of nickel chloride, 4 parts of calcium stearate, and 5 parts of sodium carboxymethyl cellulose; use a planetary mixer to add water at 19% of the total weight of the raw materials and mix and blend for 20 minutes. The weight deviation of the sand and gravel aggregate on the sieve is 9.2%.
[0065] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 45Pa, the extrusion pressure is 3.5Mpa, and the discharge speed is 12.5m / min.
[0066] S3. After molding, the green body is placed in a high-temperature autoclave for curing at 200℃ for 2 hours and 2MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0067] Example 5
[0068] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0069] S1. Add 30 parts by weight of high-silicon iron tailings, 30 parts of quicklime, 15 parts of sand and gravel aggregate, 10 parts of cement, 10 parts of polypropylene fiber, 0.5 parts of nickel chloride, 1.5 parts of calcium stearate, and 3 parts of sodium carboxymethyl cellulose.
[0070] A planetary mixer was used to add 19% water to the total weight of the raw materials and mix them for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.5%.
[0071] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 45Pa, the extrusion pressure is 3.5Mpa, and the discharge speed is 13.5m / min.
[0072] S3. After molding, the green body is placed in a high-temperature autoclave for curing at 200℃ for 2 hours and 2MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0073] Comparative Example 1
[0074] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0075] S1. Prepare the following raw materials by weight: 30 parts high-silicon iron tailings, 30 parts quicklime, 10 parts sand and gravel aggregate, 10 parts cement, 10 parts polypropylene fiber, 1 part nickel chloride, 4 parts calcium stearate, and 5 parts sodium carboxymethyl cellulose.
[0076] A planetary mixer was used, and water was added at 15% of the total weight of the raw materials. The mixture was stirred and mixed for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.1%.
[0077] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 5Pa, the extrusion pressure is 0.5Mpa, and the discharge speed is 22.1m / min.
[0078] S3. The formed green body is placed in a high-temperature autoclave for curing at 200℃ for 2 hours and 2MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0079] Comparative Example 2
[0080] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0081] S1. Prepare the following raw materials by weight: 30 parts high-silicon iron tailings, 30 parts quicklime, 10 parts sand and gravel aggregate, 10 parts cement, 10 parts polypropylene fiber, 1 part nickel chloride, 4 parts calcium stearate, and 5 parts sodium carboxymethyl cellulose.
[0082] A planetary mixer was used to add water at 15% of the total weight of the raw materials, and the mixture was stirred and mixed for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.6%.
[0083] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 15Pa, the extrusion pressure is 5Mpa, and the discharge speed is 9.5m / min.
[0084] S3. After molding, the green body is placed in a high-temperature autoclave for curing at 120°C for 1 hour and 0.5 MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0085] Comparative Example 3
[0086] A method for preparing hollow calcium silicate strips using high-silicon iron tailings and quicklime includes the following steps:
[0087] S1. Add 2 parts of sand and gravel aggregate, 3 parts of cement, 2 parts of polypropylene fiber, 0 parts of nickel chloride, 1 part of calcium stearate, and 1 part of sodium carboxymethyl cellulose to 30 parts of high silicon iron tailings and 30 parts of quicklime by weight.
[0088] A planetary mixer was used to add water at 19% of the total weight of the raw materials and mix them for 20 minutes. The weight deviation of the sand and gravel aggregates on the sieve was 9.4%.
[0089] S2. The mixed mud is shaped by extrusion. The vacuum degree of the extruder is 90Pa, the extrusion pressure is 1.5Mpa, and the discharge speed is 18.2m / min.
[0090] S3. The formed green body is placed in a high-temperature autoclave for curing at 185℃ for 1.2 hours and 1.2 MPa. After autoclaving, hollow calcium silicate strip material is obtained.
[0091] The materials prepared in the above embodiments and comparative examples were tested for compressive strength and impact resistance according to the standards and requirements of GB / T 23451-2023 Lightweight partition wall panels for building. The results are shown in Table 1.
[0092] Table 1
[0093] Compressive strength (MPa) Impact resistance (times) Example 1 14.4 25 Example 2 18.5 31 Example 3 12.6 22 Example 4 12.4 23 Example 5 12.8 19 Comparative Example 1 4.5 4 Comparative Example 2 4.1 4 Comparative Example 3 3.3 2
[0094] The difference between Example 2 and Example 1 of this invention is that in step S2 of Example 1, the extruder vacuum was reduced to 15 Pa, the extrusion pressure was increased to 5 MPa, and the discharge speed was reduced to 9.5 m / min. In step S3, the curing temperature of the autoclaving kiln was increased to 220°C, and the curing time was extended to 2 hours. The compressive strength of the prepared hollow calcium silicate strips increased to 18.5 MPa, and the impact resistance reached 31 cycles, which is more than 6 times the national standard. This indicates that the green strength is greater after the vacuum is reduced and the extrusion pressure is increased. The increased curing temperature and extended curing time result in a more complete reaction, thus improving the product strength. Conversely, in Example 3, when the vacuum was increased to 90 Pa, the extrusion pressure was reduced to 1.5 MPa, the discharge speed was increased to 18.2 m / min, the curing temperature was reduced to 185°C, and the curing time was shortened to 1.2 hours, the physical properties of the material decreased significantly. The increase in vacuum, i.e., the increase in residual gas in the material, leads to a decrease in material strength. Compared to Example 1, the study found that increasing the vacuum level and extrusion pressure increased the green density of the material by 12.2%. Increasing the curing temperature and extending the curing time resulted in a more complete hydration reaction and a 15.4% increase in the proportion of the main crystalline phase. The green density is the true density after extrusion, not the bulk density. This true density is the density of conventional materials. For porous or hollow materials, the overall density considering the pores is called bulk density; the density excluding the pores is called true density. The true density of the green is significantly affected by vacuum level, moisture content, and extrusion pressure. Lower vacuum, lower moisture content, and higher extrusion pressure result in less residual water and air in the green, leading to a higher true density. A higher true density allows for a more complete reaction during autoclaving, making crystal formation easier and increasing the proportion of the main crystalline phase. Conversely, lower true density results in lower true density.
[0095] Compared to Example 1, Comparative Example 1, with the same formulation and curing conditions, had its molding process parameters adjusted: extruder vacuum decreased to 5 Pa, extrusion pressure decreased to 0.5 MPa, and discharge speed increased to 22.1 m / min. The compressive strength of the sample decreased from 14.4 MPa to 4.5 MPa, and the number of impacts decreased from 25 to 4. The product quality could no longer meet the requirements of the current standard GB / T 23451-2023 Lightweight Partition Wall Panels for Buildings. This demonstrates that the molding process has a critical impact on product quality; exceeding the parameter control range of this invention prevents the production of high-quality products. The reason is that after the extrusion pressure was reduced during the molding process, air was not completely expelled from the sample, leaving a large number of pores. This resulted in a loose density and a significant reduction in strength after molding.
[0096] Compared to Example 2, under the same formulation conditions and molding process parameters, when the autoclaving temperature was reduced to 120°C, the curing time to 1 hour, and the curing pressure to 0.5 MPa, the compressive strength of the product decreased from 18.5 MPa to 4.1 MPa, and the number of impacts decreased from 31 to 4. This indicates that the autoclaving conditions have a significant impact on product quality. If the autoclaving parameters do not meet the control range of this invention, a product of excellent quality cannot be obtained. The reason is that the curing process is substandard, resulting in insufficient hydration reaction in the sample and failure to form effective strength.
[0097] Compared to Example 3, under the same curing conditions and molding process parameters, the proportions of stone aggregate, cement, polypropylene fiber, nickel chloride, calcium stearate, and sodium carboxymethyl cellulose in the formulation were reduced to 2 parts, 3 parts, 2 parts, 0 parts, 1 part, and 1 part, respectively. The compressive strength of the sample decreased from 12.6 MPa to 3.3 MPa, and the number of impact tests decreased from 22 to 2. This indicates that the proportion of admixtures in the formulation has a significant impact on product quality. When the amount of admixtures is reduced to the control range of this invention, a product of excellent quality cannot be obtained. This is because the admixtures promote the entire hydration reaction; too few admixtures cannot effectively promote the reaction; the hydration reaction is incomplete, resulting in insufficient strength of the resulting microstructure, which manifests as a significant reduction in the physical properties of the product.
[0098] The product prepared by the method of this invention is mainly compared with conventional interior partition wall materials such as autoclaved concrete panels, foamed ceramic panels, and extruded concrete panels. National standards exist for conventional interior partition wall materials, with a minimum compressive strength of 3.5 MPa. The current standard is GB / T 23451-2023 Lightweight Partition Wall Panels for Buildings, whose main parameters are impact resistance greater than or equal to 5 times and compressive strength greater than or equal to 4.5 MPa. Existing materials such as foamed ceramics and autoclaved aerated concrete can only achieve a maximum strength of 6 MPa. The material prepared by this invention, while being inexpensive, can achieve a strength of over 10 MPa under the same density conditions.
[0099] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any other way. Any person skilled in the art can make changes or modifications to the above-disclosed technical content to create equivalent embodiments. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A method for preparing hollow calcium silicate plates using high-silicon iron tailings and quicklime, characterized in that, It includes the following steps: S1. Using high-silicon iron tailings and quicklime as the main raw materials, sand and gravel aggregates, cement, fiber and chemical raw materials are added, and water is added and stirred and mixed. The chemical raw materials include reinforcing agents, degumming agents and plasticizers. S2. The mixed mud is shaped by extrusion. S3. After molding, the green body is cured by high-temperature steam pressure to obtain hollow calcium silicate board. In step S1, by weight, the high-silicon iron tailings are 20-30 parts, the quicklime is 20-30 parts, the sand and gravel aggregate is 10-20 parts, the cement is 10-20 parts, the fiber is 10-20 parts, the reinforcing agent is nickel chloride 0.5-1 parts, the degumming agent is calcium stearate 1-5 parts, and the plasticizer is sodium carboxymethyl cellulose 1-5 parts.
2. The method as described in claim 1, characterized in that, The main component of the ferrosilicon tailings is silicon dioxide, with a silicon dioxide content greater than 80%.
3. The method as described in claim 1, characterized in that, The main component of the quicklime is calcium oxide, with a calcium oxide content of 70-98%.
4. The method as described in claim 1, characterized in that, The fiber is one or a combination of several of the following: aluminum silicate fiber, glass wool, rock wool, and polypropylene fiber.
5. The method as described in claim 1, characterized in that, In step S1, the amount of water used is 15-19% of the total weight of the raw materials.
6. The method as described in claim 1, characterized in that, In step S1, the stirring and mixing are carried out using a planetary mixer, the mixing time is 10-30 minutes, and the weight deviation of the sieved sand and gravel aggregate is ≤10%.
7. The method as described in claim 1, characterized in that, In step S2, the extrusion molding method uses an extruder with a vacuum degree of 10-100 Pa, an extrusion pressure of 1-5 MPa, and a discharge speed of 10-20 m / min.
8. The method as described in claim 1, characterized in that, In step S3, the high-temperature autoclaving is carried out in an autoclaving kiln, the curing temperature is 195-240℃, the curing time is 2-4 hours, and the curing pressure is 1.5-2 MPa.
9. Hollow calcium silicate board prepared by the method according to any one of claims 1-8.
Citation Information
Patent Citations
Aggregate-admixture multi-solid waste fiber concrete and preparation method thereof
CN114031336A
Calcium silicate compact, and method for producing the same
JP2013203566A