Preparation method of mullite ceramic based on photocuring molding 3D printing

Through light-curing molding 3D printing technology, the problems of high cost, long cycle and low yield of complex structures in the preparation method of mullite ceramics are solved, achieving fast and high-precision production of complex-shaped ceramics, and improving the thermal stability of ceramics. and yield.

CN118771869AActive Publication Date: 2024-10-15GUILIN UNIV OF ELECTRONIC TECH +1

Patent Information

Application Number
CN202411018956.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing mullite ceramic preparation methods have high costs and long production cycles. In particular, the yield of complex structural components is low, making it difficult to manufacture mullite ceramic components with thin walls, closed cavities, and complex geometric shapes.

Method used

A method based on light-curing molding 3D printing is used to prepare silica/alumina mixed powder and light-curing printing slurry. After 3D printing, it is degreased and sintered twice, using 1,6-hexanediol diacrylate, Pentaerythritol tetraacrylate ethoxylate and dioctyl phthalate combination resin reduces viscosity and internal stress, and improves the thermal stability and density of ceramics.

Benefits of technology

It achieves rapid, customized, and high-precision production of complex-shaped mullite ceramics, improves the yield, enhances the thermal stability and creep resistance of the ceramics, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771869A_ABST
    Figure CN118771869A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of mullite ceramic based on photocuring molding 3D printing, relates to a preparation method of mullite ceramic, and aims to solve the technical problems of high cost, long production period and low finished product rate of parts with complex structures in the conventional preparation method of mullite ceramic. The method comprises the following steps: 1, preparing silicon dioxide / aluminum oxide mixed powder; 2, preparing light-cured printing slurry by using combined resin of 1, 6-hexanediol diacrylate, pentaerythritol tetraacrylate ethyoxyl ester and dioctyl phthalate; 3, carrying out 3D printing to obtain a mullite green body; 4, degreasing for two times; and 5, sintering to obtain the mullite ceramic. The printing slurry is good in stability and fluidity, the storage time can reach 10 days, the mullite phase in ceramic obtained through sintering after two times of degreasing can reach 97% or above, and the printing slurry can be used in the field of 3D printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing mullite ceramics Background Art

[0002] Mullite ceramics are used in high-temperature engineering fields due to their high melting point, creep resistance, low expansion coefficient, thermal shock resistance and excellent corrosion resistance. At the same time, mullite ceramics are also used as window materials in chemically harsh and high-temperature mechanical application environments due to their good light absorption. Existing mullite production methods include dry pressing, casting, gel injection molding, and powder injection molding. Among these methods, dry pressing and casting are mainly limited to manufacturing simpler geometric shapes. In contrast, gel casting and powder injection molding can produce complex mullite structural components. However, these two traditional molding methods belong to the category of mold manufacturing, which has high mold manufacturing costs, long production cycles, and challenges in manufacturing parts with complex shapes. For mullite ceramic parts with thin-walled structures, closed cavity structures, and complex geometric shapes, the yield rate is extremely low. Summary of the invention

[0003] The present invention aims to solve the technical problems of the existing preparation method of mullite ceramics, such as high cost, long production cycle and low yield of parts with complex structures, and provide a preparation method of mullite ceramics based on photocuring 3D printing.

[0004] The preparation method of mullite ceramics based on photocuring 3D printing of the present invention is carried out according to the following steps: 1. Preparation of silica / alumina mixed powder: adding silica powder and alumina powder in a mass ratio of 1: (3-3.2) into a ball mill for wet grinding to obtain a mixed slurry; then drying the mixed slurry and passing it through a 100-mesh sieve to obtain a silica / alumina mixed powder; 2. Preparation of photocurable printing slurry: Put silica / alumina mixed powder, resin, photoinitiator and dispersant into a ball mill, and mill them at a speed of 400-500 r / min for 400-500 min in the ball mill to obtain photocurable printing slurry; wherein, in the photocurable printing slurry, the volume of the mixed powder accounts for 30%-50% of the slurry volume; the volume of the resin accounts for 50%-70% of the slurry volume; the mass of the photoinitiator is 1%-3% of the mass of the resin; the mass of the dispersant is 1%-5% of the mass of the powder; 3. Spreading the photocurable printing slurry on a 3D photocurable printer and performing 3D printing to obtain a mullite green body; 4. Degreasing: Put the mullite green body into a tubular muffle furnace, block one end of the tubular muffle furnace, and connect the other end to an exhaust fan; use an exhaust fan to evacuate the furnace to a vacuum degree of -0.09~-0.098MPa, and at the same time, program the temperature to 480~500℃ at a heating rate of 0.5~1℃ / min and keep it for 180~200 minutes, and then cool it down to 280~300℃ at a cooling rate of 0.5~1℃ / min to complete the first step of degreasing; then turn off the exhaust fan, open both ends of the tubular muffle furnace, in an air atmosphere, program the temperature to 900~920℃ at a heating rate of 0.5~1℃ / min and keep it for 50~60 minutes, and then cool it down to 280~300℃ at a cooling rate of 0.5~1℃ / min to complete the second step of degreasing to obtain a mullite precursor; 5. Place the mullite precursor in a muffle furnace, heat it to 1600-1650°C at a heating rate of 3-5°C / min in an air atmosphere, and keep it at that temperature for 100-120 minutes for sintering to obtain mullite ceramics.

[0005] Furthermore, in the wet milling described in step 1, the ball-to-material mass ratio is 2:1; the ball milling speed is 400-500 r / min; and the ball milling time is 10-12 hours.

[0006] Furthermore, the particle size of the silicon dioxide powder described in step 1 is 400~600nm.

[0007] Furthermore, the resin in step 2 is a mixture of 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate ethoxylate and dioctyl phthalate in a volume ratio of 1: (1.5-1.6): (1-1.1).

[0008] Furthermore, the photoinitiator in step 2 is 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0009] Furthermore, the dispersant described in step 2 is dispersant S18.

[0010] Furthermore, the temperature control procedure of the first step of degreasing in step 4 is: The temperature was raised to 150 °C at a heating rate of 1 °C / min and maintained for 30 min; Then, the temperature was raised to 240-250°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 340-350°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 440-450°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Finally, the temperature was raised to 480-500°C at a heating rate of 0.5°C / min.

[0011] Furthermore, the temperature control procedure of the second step of degreasing described in step 4 is: The temperature was raised to 150 °C at a heating rate of 1 °C / min and maintained for 30 min; Then, the temperature was raised to 240-250°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 340-350°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 440-450°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature is raised to 480-500°C at a heating rate of 0.5°C / min and maintained for 100-120 minutes; Then the temperature is increased to 880~900℃ at a heating rate of 1℃ / min.

[0012] The present invention uses 1,6-hexanediol diacrylate (HDDA), pentaerythritol tetraacrylate ethoxylate (PPTTA) and dioctyl phthalate (DOP) combined resin to prepare light-cured printing slurry. Since the ceramic slurry prepared by PPTTA monomer has a large viscosity, HDDA monomer is added to reduce the viscosity of the slurry. At the same time, the added DOP molecules can be inserted between monomer molecules, thereby increasing the distance between polymers and reducing shrinkage during the polymerization process, thereby reducing the internal stress of the blank. The combination of several resins prolongs the storage time of the slurry, and the stability and fluidity of the printing slurry are good. After being stored for 10 days, it can still be printed on the machine.

[0013] The mullite green body is degreased twice to remove excess resin in the sample and avoid cracks during sintering. At the same time, the mullite phase in the sintered mullite ceramic can reach more than 97%, enhancing the thermal stability of the ceramic material, increasing the volume density, improving creep resistance and optimizing thermal insulation performance.

[0014] The method of the present invention can not only produce thin-walled structures, closed cavities and other complex geometric shapes that are difficult or impossible to achieve with traditional processes, but also has many advantages such as customization, rapid production, integration, high precision and cost-effectiveness. It can be used in the field of 3D printing. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is the XRD spectra of the ceramics obtained in Examples 1 to 5; Figure 2 is a fitting diagram of the XRD spectrum of the mullite ceramic prepared in Example 1; Figure 3 is a SEM photograph of a cross section of the mullite ceramic sample prepared in Example 1; Figure 4 This is a photo of the mullite green body of the gear obtained in step three of Example 1 and the mullite ceramic gear obtained in step five. DETAILED DESCRIPTION

[0016] The beneficial effects of the present invention are verified by the following examples.

[0017] Embodiment 1: The preparation method of mullite ceramics based on photocuring 3D printing of this embodiment is carried out according to the following steps: 1. Preparation of silica / alumina mixed powder: Add silica powder with an average particle size of 500nm and alumina powder with an average particle size of 200nm into a ball mill at a mass ratio of 1:3, and then add alcohol to make the alcohol cover the powder; finally, add grinding balls with a mass twice that of the mixed powder, and wet grind for 12 hours at a speed of 450r / min to obtain a mixed slurry; then put the mixed slurry in an oven, dry it at a temperature of 80°C for 8 hours, and then pass it through a 100-mesh sieve to obtain a silica / alumina mixed powder; 2. Preparation of photocurable printing slurry: Put silica / alumina mixed powder, resin, photoinitiator 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and dispersant S18 into a ball mill, and ball mill them at a speed of 450r / min for 500min in the ball mill to obtain photocurable printing slurry; wherein, in the photocurable printing slurry, the volume of the mixed powder accounts for 40% of the slurry volume; the volume of the resin accounts for 60% of the slurry volume; the mass of the photoinitiator is 2% of the mass of the resin; the mass of the dispersant is 3% of the mass of the powder; the resin is a mixture of 28% of 1,6-hexanediol diacrylate, 42% of pentaerythritol tetraacrylate ethoxylate and 30% of dioctyl phthalate in volume percentage; 3. Using 3D printing, spread the photocurable printing slurry in the resin tank of the CeraRay TC-I ceramic 3D printer, set the layer thickness to 100 μm, and the printing speed to 20 s / layer to perform 3D printing to obtain the mullite green body of the gear; 4. Degreasing: Put the mullite green body into a tubular muffle furnace, plug one end of the tubular muffle furnace, and connect the other end to an exhaust fan; use the exhaust fan to evacuate the furnace to a vacuum degree of -0.09~-0.098MPa, and at the same time, heat up to 150℃ at a heating rate of 1℃ / min and keep it for 30 minutes; then heat up to 250℃ at a heating rate of 0.5℃ / min and keep it for 60 minutes; then heat up to 350℃ at a heating rate of 0.5℃ / min and keep it for 60 minutes; then heat up to 450℃ at a heating rate of 0.5℃ / min and keep it for 60 minutes; finally, heat up to 500℃ at a heating rate of 0.5℃℃ / min and keep it for 180 minutes, and then cool down to 300℃ at a cooling rate of 1℃ / min to complete the first step of degreasing; Then turn off the exhaust fan, open both ends of the tubular muffle furnace, and in an air atmosphere, heat up to 150°C at a heating rate of 1°C / min and keep for 30 minutes; then heat up to 250°C at a heating rate of 0.5°C / min and keep for 60 minutes; then heat up to 350°C at a heating rate of 0.5°C / min and keep for 60 minutes; then heat up to 450°C at a heating rate of 0.5°C / min and keep for 60 minutes; then heat up to 500°C at a heating rate of 0.5°C / min and keep for 120 minutes; then heat up to 900°C at a heating rate of 1°C / min and keep for 60 minutes, and then cool down to 300°C at a cooling rate of 1°C / min, completing the second step of degreasing to obtain a mullite precursor; 5. Place the mullite precursor in a muffle furnace, heat it to 1000°C at a heating rate of 5°C / min in an air atmosphere, and then heat it to 1650°C at a rate of 3°C / min and keep it for 120 minutes for sintering to obtain a mullite ceramic gear.

[0018] Example 2: This example is different from Example 1 in that the sintering temperature in step five is 1300° C., and the rest is the same as Example 1.

[0019] Example 3: This example is different from Example 1 in that the sintering temperature in step five is 1400° C., and the rest is the same as Example 1.

[0020] Example 4: This example is different from Example 1 in that the sintering temperature in step five is 1500° C., and the rest is the same as Example 1.

[0021] Example 5: This example is different from Example 1 in that the sintering temperature in step five is 1600° C., and the rest is the same as Example 1.

[0022] The ceramics obtained in Examples 1 to 5 were subjected to X-ray diffraction spectrum testing, and the obtained XRD spectra were as follows: Figure 1 As shown, from Figure 1It can be seen that the mullite phase does not appear in the samples sintered at 1300℃ and 1400℃, and the mullite phase begins to appear at 1500℃, but is accompanied by alumina and silica phases. At 1600℃ and 1650℃, the mullite phase has become the main phase, with some alumina phase remaining.

[0023] The XRD spectrum of the mullite ceramic prepared in Example 1 is as follows: Figure 2 As shown, by fitting it, the phase contents can be obtained as follows: the mullite content is 97.65wt%, and the alumina content is 2.35wt%.

[0024] The cross section of the mullite ceramic sample prepared in Example 1 was scanned by SEM, and the obtained SEM photo is as follows: Figure 3 As shown, from Figure 3 It can be found that the density of the sample is relatively high.

[0025] Figure 4 The mullite green body of the gear obtained in step 3 of Example 1 and the photo of the mullite ceramic gear obtained in step 5 are shown in FIG. Figure 4 It can be seen that the sample shrinks after sintering at 1650° and the density increases.

[0026] Comparative Example 1: This comparative example is different from Example 1 in that the average particle size of the silicon dioxide powder in step 1 is 200 nm, the average particle size of the aluminum oxide powder is 200 nm, and the other steps and parameters are the same as those in Example 1.

[0027] Since the particle size of the powder in this comparative example 1 is too small, the small particles provide a larger surface area, which increases the internal friction of the slurry, deteriorates the fluidity, and increases the viscosity of the slurry; at the same time, the slurry prepared under this condition has a low curing depth due to its high viscosity, making it difficult to cure, thereby affecting the bonding strength between the printed layers; in addition, the ceramic prepared in this comparative example 1 will crack.

[0028] Comparative Example 2: This comparative example is different from Example 1 in that in step 1, the average particle size of the silicon dioxide powder is 1000 nm, and the average particle size of the aluminum oxide powder is 200 nm. The other steps and parameters are the same as those in Example 1.

[0029] Since the particle size of the silicon dioxide powder in this comparative example is too large, the mechanical strength of the printed sample decreases after sintering, the density is low, and the mullite phase content in the ceramic sample is reduced.

[0030] Comparative Example 3: This comparative example is different from Example 1 in that the resin in step 2 is 100% 1,6-hexanediol diacrylate. Other steps and parameters are the same as those in Example 1.

[0031] The resin in this comparative example is single 1,6-hexanediol diacrylate, and the prepared slurry has a poor preservation effect and the slurry settles after 1 day.

[0032] Comparative Example 4: This comparative example is different from Example 1 in that the resin in step 2 is 100% ethoxylated pentaerythritol tetraacrylate (PPTTA), and the other steps and parameters are the same as those in Example 1.

[0033] The resin in this comparative example is single PPTTA, and the viscosity of the PPTTA resin is too large and the fluidity is poor.

[0034] Comparative Example 5: This comparative example is different from Example 1 in that the resin in step 2 is a mixture of 50% 1,6-hexanediol diacrylate and 50% PPTTA by volume, and the other steps and parameters are the same as Example 1.

[0035] In the resin of this comparative example, dioctyl phthalate (DOP) was not added, and the sample was severely cracked after degreasing.

[0036] Comparative Example 6: This comparative example is different from Example 1 in that the first degreasing is omitted in step 4, and only the second degreasing is performed. The other steps and parameters are the same as those in Example 1.

[0037] In this comparative example, only degreasing in air was performed, and the resin in the sample was not completely removed, resulting in cracking after sintering.

Claims

1. A method for preparing mullite ceramics based on photocuring 3D printing, characterized in that The method proceeds as follows:

1. Preparation of silica / alumina mixed powder: adding silica powder and alumina powder in a mass ratio of 1: (3-3.2) into a ball mill for wet grinding to obtain a mixed slurry; then drying the mixed slurry and passing it through a 100-mesh sieve to obtain a silica / alumina mixed powder; 2. Preparation of photocurable printing slurry: Put silica / alumina mixed powder, resin, photoinitiator and dispersant into a ball mill, and mill them at a speed of 400-500 r / min for 400-500 min in the ball mill to obtain photocurable printing slurry; wherein, in the photocurable printing slurry, the volume of the mixed powder accounts for 30%-50% of the slurry volume; the volume of the resin accounts for 50%-70% of the slurry volume; the mass of the photoinitiator is 1%-3% of the mass of the resin; the mass of the dispersant is 1%-5% of the mass of the powder; 3. Spreading the photocurable printing slurry on a 3D photocurable printer and performing 3D printing to obtain a mullite green body; 4. Degreasing: Put the mullite green body into a tubular muffle furnace, block one end of the tubular muffle furnace, and connect the other end to an exhaust fan; use an exhaust fan to evacuate the furnace to a vacuum degree of -0.09~-0.098MPa, and at the same time, program the temperature to 480~500℃ at a heating rate of 0.5~1℃ / min and keep it for 180~200 minutes, and then cool it down to 280~300℃ at a cooling rate of 0.5~1℃ / min to complete the first step of degreasing; then turn off the exhaust fan, open both ends of the tubular muffle furnace, in an air atmosphere, program the temperature to 900~920℃ at a heating rate of 0.5~1℃ / min and keep it for 50~60 minutes, and then cool it down to 280~300℃ at a cooling rate of 0.5~1℃ / min to complete the second step of degreasing to obtain a mullite precursor; 5. Place the mullite precursor in a muffle furnace, heat it to 1600-1650°C at a heating rate of 3-5°C / min in an air atmosphere, and keep it at that temperature for 100-120 minutes for sintering to obtain mullite ceramics.

2. The method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1, characterized in that: In the wet milling described in step 1, the ball-to-material mass ratio is 2:1; the ball milling speed is 400-500 r / min; and the ball milling time is 10-12 hours.

3. A method for preparing mullite ceramics based on photocuring 3D printing according to claim 1 or 2, characterized in that: The particle size of the silicon dioxide powder described in step 1 is 400-600 nm.

4. A method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1 or 2, characterized in that: The resin described in step 2 is a mixture of 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate ethoxylate and dioctyl phthalate in a volume ratio of 1: (1.5-1.6): (1-1.1).

5. A method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1 or 2, characterized in that: The photoinitiator described in step 2 is 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

6. A method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1 or 2, characterized in that: The dispersant described in step 2 is dispersant S18.

7. A method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1 or 2, characterized in that: The temperature control procedure for the first step of degreasing described in step 4 is: The temperature was raised to 150 °C at a heating rate of 1 °C / min and maintained for 30 min; Then, the temperature was raised to 240-250°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 340-350°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 440-450°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Finally, the temperature was raised to 480-500°C at a heating rate of 0.5°C / min.

8. A method for preparing mullite ceramics based on photo-stereolithography 3D printing according to claim 1 or 2, characterized in that: The temperature control procedure for the second step of degreasing described in step 4 is: The temperature was raised to 150 °C at a heating rate of 1 °C / min and maintained for 30 min; Then, the temperature was raised to 240-250°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 340-350°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature was raised to 440-450°C at a heating rate of 0.5°C / min and maintained for 50-60 minutes; Then, the temperature is raised to 480-500°C at a heating rate of 0.5°C / min and maintained for 100-120 minutes; Then the temperature is increased to 880~900℃ at a heating rate of 1℃ / min.

Citation Information

Patent Citations

  • Indirect free forming method for complex ceramic structural parts

    CN110143819A

  • Preparation method of light-cured silicon nitride ceramic slurry and silicon nitride ceramic

    CN114524676A

  • Preparation method of mullite infrared transparent ceramic

    CN114644513A

  • High-complexity ceramic component and preparation method thereof

    CN116553918A

  • High-solid-content silicon nitride ceramic slurry, silicon nitride ceramic and preparation method

    CN117819990A

Cited By

  • Preparation method of microwave dielectric ceramic material based on photocuring 3D printing

    CN119613113A

  • Photocuring printing mother-of-pearl alumina composite ceramic based on alumina lamellar crystal adsorption SiO2 and method

    CN119797895A

  • Surface-modified aluminum oxide nanoparticles as well as preparation method and application thereof

    CN121063917A