Photocuring 3D printing ceramic-polymer slurry based on aluminum sol coating method and preparation method thereof
By modifying the surface of SiC powder using an aluminum sol coating method, a low-viscosity, high-solid-content photopolymer slurry for photocuring 3D printing was prepared. This solved the problems of light penetration depth and interface defects in the photocuring process of non-oxide ceramic powder, thus improving printing quality and performance.
Patent Information
- Application Number
- CN202410828559.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-01
AI Technical Summary
In the process of photopolymerization 3D printing, non-oxide ceramic powders have a high refractive index and high light absorption, which reduces the light penetration depth, affects curing efficiency and product quality, and causes interface defects such as bubbles, cracks or delamination.
SiC powder was surface modified by aluminum sol coating to prepare SiC@Al2O3 composite powder, which was then combined with photosensitive resin, dispersant and photoinitiator to form a low-viscosity, high-solid-content photocurable 3D printing ceramic-polymer slurry.
It reduces the absorbance and refractive index of SiC powder, increases the solid content and mechanical properties of photopolymer 3D printing, reduces printing defects, and improves the surface quality and optical properties of products.
Smart Images

Figure CN118878331A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ceramic photocuring 3D printing, and specifically relates to a photocuring 3D printing ceramic-polymer slurry based on an aluminum sol coating method and a preparation method thereof. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] Ceramic materials are widely used in aerospace, biomedicine, electronic information and other industries due to their excellent high-temperature strength, wear resistance, corrosion resistance and good thermal insulation properties. However, traditional ceramic manufacturing processes often have problems such as difficult processing, high cost and long production cycle, which limit the further application and development of ceramic materials. In recent years, researchers have successfully prepared a variety of ceramic-polymer slurries, including alumina (Al2O3), zirconium oxide (ZrO2), silicon carbide (SiC), etc. through 3D printing technology, especially stereolithography (SLA) technology.
[0004] Silicon carbide (SiC) ceramics are structural ceramic materials with high thermal conductivity, low thermal expansion coefficient and high mechanical strength. However, this non-oxide ceramic faces some challenges in stereolithography (SLA) technology, mainly due to the physical properties of this type of material, especially the high refractive index and absorbance, which affect the propagation and curing efficiency of ultraviolet light during the photocuring process. The main problem at present is that during printing, the high refractive index non-oxide ceramic powder will absorb and scatter ultraviolet light, resulting in a decrease in the penetration depth of light during the photocuring process, limiting the increase in the solid content of the slurry. After printing, interface defects such as bubbles, cracks or delamination may be formed during the curing process, which will affect the mechanical properties and surface quality of the final product. The high absorbance of non-oxide ceramic powders can also cause local overheating or uneven curing of the photocurable resin, affecting the overall optical properties and transparency of the slurry, which is particularly important for applications requiring high optical quality. Summary of the invention
[0005] In order to reduce the refractive index and absorbance of non-oxide ceramics, thereby improving the solid content and curing effect of photocurable 3D printing ceramic-polymer slurry, reducing printing interface defects, and improving mechanical properties and surface quality. The present invention proposes a photocurable 3D printing ceramic-polymer slurry based on an aluminum sol coating method and a preparation method thereof, which is used to reduce the absorbance and viscosity of non-oxide ceramic-polymer slurry, thereby improving the solid content and comprehensive performance of non-oxide ceramic-polymer slurry in photocurable 3D printing.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a photocurable 3D printing ceramic-polymer slurry based on an aluminum sol coating method, comprising the following steps:
[0008] Adding the aluminum oxide precursor and the catalyst dropwise into water, mixing evenly, heating and stirring, and preparing the boehmite sol;
[0009] SiC powder is added into boehmite sol, mixed evenly, and subjected to heating reaction, drying, grinding and sintering to obtain SiC@Al2O3 composite powder;
[0010] The SiC@Al2O3 composite powder is mixed with a photosensitive resin, a dispersant and a photoinitiator to obtain a photocurable 3D printing ceramic-polymer slurry.
[0011] In some embodiments, the aluminum oxide precursor is a metal alkoxide, acetate or oxalate of aluminum;
[0012] Preferably, the aluminum oxide precursor is aluminum isopropoxide, aluminum butoxide or aluminum oxalate.
[0013] In some embodiments, the catalyst is an acid or a base, the acid is selected from one of hydrochloric acid, sulfuric acid, nitric acid or acetic acid or a mixture thereof; the base is one of ammonia water and sodium hydroxide or a mixture thereof.
[0014] In some embodiments, the concentration of the catalyst is 0.1-2 mol / L.
[0015] In some embodiments, the temperature of heating and stirring is 50-60° C., and the rotation speed is 300-400 r / min.
[0016] In some embodiments, the SiC powder is an amorphous powder, and the powder particle size is 0.5-10 μm.
[0017] Preferably, in the SiC@Al2O3 composite powder, the mass ratio of SiC to Al2O3 is 1:1-5.
[0018] In some embodiments, the temperature of the heating reaction is 80-90° C., and the heating reaction time is 1-2 hours.
[0019] Preferably, during the heating reaction, the stirring speed is 400-500 r / min.
[0020] In some embodiments, the drying is vacuum drying, the vacuum drying temperature is 80-120° C., and the drying time is greater than 6 hours.
[0021] Preferably, the solid product obtained after drying is crushed, ground, and passed through a 100-mesh sieve to obtain a uniform powder.
[0022] In some embodiments, the sintering is performed in an inert atmosphere.
[0023] Preferably, the sintering procedure is:
[0024] At room temperature, heat up to 450℃ at 5-10℃ and keep warm for 15h;
[0025] On the basis of 450℃, increase the temperature by 2~5℃ to 900~1200℃ and keep it warm for 90min;
[0026] The sintered body is naturally cooled in the tube furnace for 5 to 10 hours.
[0027] Room temperature refers to the ambient temperature, which is 20-30°C.
[0028] In some embodiments, in the photocurable 3D printing ceramic-polymer slurry, the mass fraction of the powder is 40-60wt%, the mass fraction of the photosensitive resin is 20-36wt%, and the mass fraction of the dispersant is 2-6wt%.
[0029] Preferably, the photosensitive resin is selected from one of 1,6-hexanediol diacrylate HDDA, trimethylolpropane triacrylate TMPTA, and acryloyl morpholine ACMO, or a combination thereof.
[0030] Preferably, the dispersant is selected from one or a combination of KOS110, KOS163 or KOS200.
[0031] In some embodiments, the photoinitiator is one of TPO, 819 or 184 or a combination thereof.
[0032] In a second aspect, the present invention provides a photocurable 3D printing ceramic-polymer slurry based on an aluminum sol coating method, which is prepared by the preparation method.
[0033] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0034] By using powder surface modification technology to change the surface state of the powder and reduce the refractive index and absorbance of high refractive index and absorbance ceramic materials, a photocurable ceramic-polymer slurry system with high solid content, low viscosity and strong stability for actual photocurable 3D printing can be prepared. The process of the invention is simple to operate, short in preparation time, low in production cost, and has a significant improvement effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0036] Figure 1It is a process flow chart of preparing SLA light-cured 3D printing ceramic-polymer slurry by the aluminum sol coating method according to an embodiment of the present invention;
[0037] Figure 2 is a sintering process diagram of an embodiment of the present invention;
[0038] Figure 3 It is a rheological property test chart of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0039] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0040] The specific method for preparing SLA light-cured 3D printing ceramic-polymer slurry in the present invention is described in detail below, and a light-cured ceramic-polymer slurry with high solid content, low viscosity and strong stability can be obtained. The present invention is further described below in conjunction with examples.
[0041] Example 1
[0042] A SLA photocuring 3D printing ceramic-polymer slurry using an aluminum sol coating method, the mass fraction percentage (wt %) is shown in Table 1.
[0043] Table 1 Ceramic-polymer slurry mass percentage (wt%)
[0044] <![CDATA[SiC@Al2O3]]> Photosensitive resin Dispersants Photoinitiator 60wt% 36wt% 4wt% 2% (relative to the total mass of resin)
[0045] 5 g of aluminum isopropoxide and 5 g of nitric acid (0.5 mol / L) were slowly dropped into 40 g of deionized water and mixed evenly. The mixture was heated and stirred using a magnetic stirrer at a heating temperature of 60° C., a rotation speed of 400 r / min, and a stirring time of 2 h until a boehmite sol was formed.
[0046] 5 g of SiC powder with a particle size of 0.5 to 10 μm was added to the boehmite sol, the temperature was raised to 80° C., and magnetic stirring was continued for 2 h at a speed of 400 r / min to obtain a SiC@Al2O3 composite powder mixture.
[0047] The SiC@Al2O3 composite powder mixture was placed in a drying oven and vacuumed, the heating temperature was 80-120°C, and the drying time was greater than 8 hours. The dried SiC@Al2O3 composite powder was transferred to a mortar, and crushed in the mortar at room temperature to pass through a 100-mesh sieve to obtain a uniform powder.
[0048] The sintering was carried out in a tubular furnace, and Ar was introduced as a protective gas. The specific sintering procedure is as follows: In the first stage, at room temperature, the temperature was raised to 450°C at a first heating rate of 5°C and then kept at this temperature for 15 hours. In the second stage, based on 450°C, the temperature was raised to 1200°C at a second heating rate of 3°C and kept at this temperature for 90 minutes. In the third stage, after the holding time, the sintered body was naturally cooled in the tubular furnace for 10 hours. The above temperature sintering curves are shown in Figure 1. Figure 2 shown.
[0049] Photosensitive resin TMPTA, dispersant KOS163 and photoinitiator TPO were added to the SiC@Al2O3 composite powder in the above proportions, and then stirred using a magnetic stirrer for 30 minutes at a speed of 350 rpm to test the rheological properties of the ceramic-polymer slurry.
[0050] Comparative Example 1
[0051] A SLA light-curing 3D printing ceramic-polymer slurry, the mass percentage (wt %) is shown in Table 2.
[0052] Table 2 Ceramic-polymer slurry mass ratio (wt%)
[0053] SiC Photosensitive resin Dispersants Photoinitiator 60wt% 36wt% 4wt% 2% (relative to the total mass of resin)
[0054] This comparative example 1 is different from the example 1 in that the powder material in the example 1 is modified by the aluminum sol coating method, while in the comparative example 1, 0.5-10 μm SiC powder is directly added to the photosensitive resin, dispersant and photoinitiator, and then the ceramic-polymer slurry is prepared by stirring with a magnetic stirrer for 30 min (350 rpm), and the rheological properties of the ceramic-polymer slurry are tested. Figure 3 .
[0055] Comparative Example 2
[0056] A SLA light-curing 3D printing ceramic-polymer slurry, the mass percentage (wt %) is shown in Table 3.
[0057] Table 3 Ceramic-polymer slurry mass ratio (wt%)
[0058] <![CDATA[Al2O3]]> Photosensitive resin Dispersants Photoinitiator 60wt% 36wt% 4wt% 2% (relative to the total mass of resin)
[0059] Comparative Example 2 is different from Example 1 in that the powder material in Example 1 is modified by the aluminum sol coating method, while in Comparative Example 2, 0.5-10 μm Al2O3 powder is directly added to the photosensitive resin, dispersant and photoinitiator, and then stirred with a magnetic stirrer for 30 min (350 rpm) to prepare a ceramic-polymer slurry, and the rheological properties of the ceramic-polymer slurry are tested. Figure 3 .
[0060] Comparative Example 3
[0061] A SLA light-curing 3D printing ceramic-polymer slurry, the mass percentage (wt %) is shown in Table 4.
[0062] Table 4 Ceramic-polymer slurry mass ratio (wt%)
[0063]
[0064] This comparative example 3 is different from the example 1 in that the powder material in the example 1 is modified by the aluminum sol coating method, while in the comparative example 3, 0.5-10 μm SiC powder and 0.5-10 μm Al2O3 powder (mass ratio is 1:1) are directly added to the photosensitive resin, dispersant and photoinitiator, and then the ceramic-polymer slurry is prepared by stirring with a magnetic stirrer for 30 min (350 rpm), and the rheological properties of the ceramic-polymer slurry are tested. Figure 3 .
[0065] according to Figure 3 It can be seen that at a shear rate of 30 -1 s, the viscosity of the ceramic-polymer slurry prepared with SiC@Al2O3 composite powder in Example 1 is 240mPa·s; the viscosity of the ceramic-polymer slurry prepared with SiC powder in Comparative Example 1 is 840mPa·s; the viscosity of the ceramic-polymer slurry prepared with Al2O3 powder in Comparative Example 2 is 244mPa·s; the viscosity of the ceramic-polymer slurry prepared with SiC:Al2O3 (mass ratio of 1:1) mixed powder in Comparative Example 3 is 360mPa·s. From the viscosity data, it can be found that the viscosity of the ceramic-polymer slurry prepared with SiC@Al2O3 composite powder in Example 1 decreases significantly, and is not much different from the viscosity of the ceramic-polymer slurry prepared with Al2O3 powder in Comparative Example 2. At a shear rate of 30 -1 s time gap 4mPa·s, shear rate 60 -1 s, the gap is 8mPa·s. It can be seen that the ceramic-polymer slurry prepared by the aluminum sol-coated powder modification method has a low viscosity, which provides a new solution for the preparation of high solid content light-curing 3D printing ceramic-polymer slurry in the future.
[0066] Table 5 Absorbance data comparison
[0067] name Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Absorbance 1.341 1.386 1.291 1.380
[0068] Table 5 shows the absorbance data of Example 1 and Comparative Examples 1, 2, and 3 at a wavelength of 355 nm. It can be seen from the data in the table that the absorbance of Example 1 is reduced by 0.045 compared with the absorbance in Comparative Example 1, indicating that the surface modification of SiC powder by aluminum sol coating method can effectively reduce the absorbance of the SiC powder surface, thereby improving the printing effect of ceramic-polymer slurry.
[0069] Alumina powder is white with a refractive index of about 1.7, and silicon carbide powder is gray-green with a refractive index of about 2.7. From the absorbance data, it can be seen that the absorbance in Example 1 is reduced, indicating that aluminum oxide is coated on the surface of silicon carbide, thereby reducing the refractive index of silicon carbide.
[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a photocurable 3D printing ceramic-polymer slurry based on an aluminum sol coating method, characterized in that: The steps include: Adding the aluminum oxide precursor and the catalyst dropwise into water, mixing evenly, heating and stirring, and preparing the boehmite sol; SiC powder is added into boehmite sol, mixed evenly, and subjected to heating reaction, drying, grinding and sintering to obtain SiC@Al2O3 composite powder; The SiC@Al2O3 composite powder is mixed with a photosensitive resin, a dispersant and a photoinitiator to obtain a photocurable 3D printing ceramic-polymer slurry.
2. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The aluminum oxide precursor is aluminum metal alkoxide, acetate or oxalate; Preferably, the aluminum oxide precursor is aluminum isopropoxide, aluminum butoxide or aluminum oxalate.
3. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The catalyst is an acid or a base, wherein the acid is selected from hydrochloric acid, sulfuric acid, nitric acid or acetic acid or a mixture thereof; the base is ammonia water, sodium hydroxide or a mixture thereof.
4. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The temperature of heating and stirring is 50-60°C, and the speed is 300-400r / min; Preferably, the SiC powder is an amorphous powder with a particle size of 0.5 to 10 μm; Preferably, in the SiC@Al2O3 composite powder, the mass ratio of SiC to Al2O3 is 1:1-5.
5. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The temperature of the heating reaction is 80-90° C., and the time of the heating reaction is 1-2 hours. Preferably, during the heating reaction, the stirring speed is 400-500 r / min.
6. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The drying is vacuum drying, the vacuum drying temperature is 80-120°C, and the drying time is greater than 6 hours; Preferably, the solid product obtained after drying is crushed, ground, and passed through a 100-mesh sieve to obtain a uniform powder.
7. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The sintering is carried out in an inert atmosphere; Preferably, the sintering procedure is: At room temperature, heat up to 450℃ at 5-10℃ and keep warm for 15h; On the basis of 450℃, increase the temperature by 2~5℃ to 900~1200℃ and keep it warm for 90min; The sintered body is naturally cooled in the tube furnace for 5 to 10 hours.
8. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: In the photocurable 3D printing ceramic-polymer slurry, the mass fraction of SiC@Al2O3 composite powder is 40-60wt%, the mass fraction of photosensitive resin is 20-36wt%, and the mass fraction of dispersant is 2-6wt%; Preferably, the photosensitive resin is selected from one of 1,6-hexanediol diacrylate HDDA, trimethylolpropane triacrylate TMPTA, and acryloyl morpholine ACMO, or a combination thereof.
9. The method for preparing a light-cured 3D printing ceramic-polymer slurry based on an aluminum sol coating method according to claim 1, characterized in that: The dispersant is selected from one or a combination of KOS110, KOS163 or KOS200; Alternatively, the photoinitiator is one of TPO, 819 or 184 or a combination thereof.
10. A photocurable 3D printing ceramic-polymer slurry based on an aluminum sol coating method, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of difficult-to-cure ceramic based on photocuring forming and product
CN113880559A
ceramic slurry composition with low viscosity for 3D printing
KR1020150077649A
Cited By
Method for preparing porous ceramic by photocuring sol-modified SiC particles
CN119638483A
Preparation method of multi-component photocuring composite ceramic
CN120864893A
High-formability and high-volume-fraction SiC / AlSi10Mg composite material and additive manufacturing method thereof