Modified hydrogel electrolyte for quasi-solid-state zinc ion battery and preparation method of modified hydrogel electrolyte

By introducing polyvinyl alcohol and tetramethylurea into the hydrogel electrolyte, the problems of zinc anode corrosion and low-temperature performance in zinc-ion batteries are solved, the mechanical properties and low-temperature performance of the electrolyte are improved, the battery life is extended, and it is suitable for large-scale Production.

CN118772445APending Publication Date: 2024-10-15SICHUAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411256231.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional aqueous zinc-ion batteries have problems with zinc anode corrosion and hydrogen evolution reaction, which lead to shortened battery life and reduced conductivity at low temperature. Existing modification methods have problems such as reduced conductivity, increased costs, and environmental pollution.

Method used

Polyvinyl alcohol and tetramethylurea are introduced into the hydrogel electrolyte, and the modified hydrogel electrolyte is prepared through steps such as heating and dissolving in a water bath, low-temperature freezing, and vacuum drying to improve mechanical properties and corrosion resistance, and regulate the solvation structure of zinc ions. , breaking the hydrogen bonds between free water molecules.

Benefits of technology

It significantly improves the mechanical properties, corrosion resistance and low-temperature performance of the electrolyte, extends the cycle performance and service life of zinc-ion batteries, and is suitable for large-scale production and practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772445A_ABST
    Figure CN118772445A_ABST
Patent Text Reader

Abstract

The invention discloses a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery and a preparation method of the modified hydrogel electrolyte, and relates to the technical field of hydrogel electrolytes.The preparation method comprises the following steps that a corresponding aqueous solution of zinc trifluoromethanesulfonate is provided; dissolving polyvinyl alcohol particles in a zinc salt aqueous solution under the conditions of water bath heating and stirring; adding tetramethylurea in different proportions into the polyvinyl alcohol hydrogel electrolyte prepared in the step S2, and heating and stirring to obtain a uniformly mixed viscous solution; freezing the obtained viscous solution at a low temperature for more than 12 hours; and taking out the obtained electrolyte, cooling to room temperature, and carrying out vacuum drying to obtain the functional hydrogel electrolyte. The polyvinyl alcohol and the tetramethylurea are introduced into the hydrogel electrolyte, so that the mechanical property and the corrosion resistance of the electrolyte are remarkably improved. The polyvinyl alcohol has good film-forming property and mechanical strength, so that the electrolyte material can better resist physical stress and chemical corrosion in the use process, thereby prolonging the service life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogel electrolytes, in particular to a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery and a preparation method thereof. Background Art

[0002] Against the backdrop of the global energy crisis and increasing environmental pollution, the development of efficient and clean energy storage and conversion systems has become an important issue in today's society. As an important energy storage device, lithium-ion batteries (LIBs) have been widely used in portable electronic devices, electric vehicles, and energy storage power stations due to their high energy density and long cycle life. However, the organic electrolytes used in lithium-ion batteries are flammable and chemically unstable, which makes them prone to combustion or explosion under extreme conditions such as high temperature and overcharging, posing a major safety hazard. In addition, the limited and uneven distribution of lithium resources also make lithium-ion batteries more expensive, restricting their promotion and application on a larger scale.

[0003] Compared with lithium-ion batteries, zinc-ion batteries (ZIBs) have attracted widespread attention in recent years due to their high safety, abundant raw materials, low cost and environmental friendliness. Zinc, as the negative electrode material of the battery, has a high theoretical capacity (820mAh / g) and a low redox potential (-0.76 V vs. SHE). Zinc resources are abundant and inexpensive. However, traditional aqueous zinc-ion batteries use aqueous electrolytes. Although they are highly conductive and environmentally friendly, they still have a series of problems that need to be solved.

[0004] First, the aqueous electrolyte in the aqueous zinc-ion battery easily causes corrosion and hydrogen evolution reaction of the zinc negative electrode. This is because zinc easily reacts with water molecules in aqueous solution to generate hydrogen, which causes the zinc negative electrode to be gradually consumed and the battery life to be greatly shortened. In addition, the aqueous electrolyte is easy to freeze at low temperatures, which significantly reduces the migration rate of zinc ions in the electrolyte, thus affecting the low-temperature performance of the battery.

[0005] In order to solve these problems, researchers have proposed a variety of modification methods, including the introduction of electrolyte additives, the development of organic electrolytes and ionic liquid electrolytes, etc. For example, adding certain organic additives to aqueous electrolytes can effectively inhibit the corrosion and hydrogen evolution reaction of the zinc negative electrode and improve the cycle stability of the battery; using organic electrolytes or ionic liquid electrolytes can avoid the presence of water molecules to a certain extent, thereby reducing the corrosion and hydrogen evolution reaction of the zinc negative electrode. However, these modification methods are often accompanied by problems such as decreased conductivity, increased costs and environmental pollution.

[0006] In this context, hydrogel electrolytes, as a new type of electrolyte material, have gradually attracted the attention of researchers. Hydrogel is a three-dimensional network structure composed of a hydrophilic polymer network and a large number of water molecules, with excellent ionic conductivity and good mechanical properties. Hydrogel electrolytes not only provide ionic conductivity comparable to aqueous electrolytes, but also have the dimensional stability of solid electrolytes, which can effectively prevent electrolyte leakage and significantly improve battery safety. In addition, the water molecules in the hydrogel electrolyte are bound by the polymer network and are not easy to freeze, allowing the battery to work normally at low temperatures.

[0007] Although hydrogel electrolytes have shown great potential in improving the performance of zinc-ion batteries, current research still faces some challenges, such as how to further improve the ionic conductivity, mechanical properties and environmental stability of hydrogel electrolytes; how to achieve large-scale application of hydrogel electrolytes in zinc-ion batteries by optimizing electrolyte composition and preparation process.

[0008] In view of the above problems, the present invention provides a modified hydrogel electrolyte and a preparation method thereof. By introducing polyvinyl alcohol and tetramethyl urea into the hydrogel electrolyte, the mechanical properties and corrosion resistance of the electrolyte can be significantly improved while maintaining good ionic conductivity and low temperature performance. Polyvinyl alcohol, as a commonly used water-soluble polymer, has excellent film-forming properties and mechanical strength; tetramethyl urea is an organic compound containing oxygen groups, which can interact with water molecules, polyvinyl alcohol and zinc ions, thereby regulating the solvation structure of zinc ions, breaking the hydrogen bonds between free water molecules, and reducing the activity of water.

[0009] The preparation method of the modified hydrogel electrolyte of the present invention is simple and easy. Through the steps of water bath heating dissolution, low temperature freezing and vacuum drying, a hydrogel electrolyte with excellent performance can be prepared. The specific steps are as follows: first, a certain amount of zinc trifluoromethanesulfonate is dissolved in deionized water to form a uniform zinc salt solution; then, polyvinyl alcohol particles are added to the zinc salt solution under the condition of water bath heating and stirring until it is completely dissolved; then, tetramethyl urea of ​​different proportions is added, and a uniformly mixed viscous solution is obtained by heating and stirring; the viscous solution is frozen at low temperature for more than 12 hours, taken out and cooled to room temperature, and finally dried under vacuum drying conditions to obtain a stable functional hydrogel electrolyte with good corrosion resistance.

[0010] The modified hydrogel electrolyte material of the present invention not only has good mechanical properties and corrosion resistance, but also has excellent low temperature performance and environmental stability, and can be well applied in practical environments. The functional hydrogel electrolyte prepared by the above modification method can significantly improve the cycle performance and service life of zinc ion batteries, and has broad application prospects. Summary of the invention

[0011] Based on the existing technical problems, the present invention proposes a method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery, comprising the following steps: S1: providing a corresponding aqueous solution of zinc trifluoromethanesulfonate; S2: dissolving the polyvinyl alcohol particles by heating and stirring the zinc salt aqueous solution in a water bath; S3: adding tetramethyl urea in different ratios to the polyvinyl alcohol hydrogel electrolyte prepared in S2, and obtaining a uniformly mixed viscous solution by heating and stirring; S4: freezing the obtained viscous solution at low temperature for more than 12 hours; S5: Take out the obtained electrolyte, cool it to room temperature and then vacuum dry it to obtain a stable functional hydrogel electrolyte with good corrosion resistance.

[0012] As a preferred technical solution of the present invention, the volume ratio of tetramethyl urea to water in S3 is 1:20, 1:10, and 1:5; the amount of polyvinyl alcohol is 3 g, and the concentration of zinc trifluoromethanesulfonate is 2 mol / L.

[0013] As a preferred technical solution of the present invention, the conditions for water bath heating and stirring in S2 are 80-90°C and the rotation speed is 100-500r / min.

[0014] As a preferred technical solution of the present invention, the low temperature condition in S4 is -15°C.

[0015] As a preferred technical solution of the present invention, the degree of polymerization of the polyvinyl alcohol is 1750±50, and the degree of alcoholysis is 98%±1%.

[0016] As a preferred technical solution of the present invention, the dissolution time of the polyvinyl alcohol particles in S2 is 5 to 10 hours.

[0017] As a preferred technical solution of the present invention, the added amount of tetramethyl urea in S3 is 0.5 mL, 1.0 mL, and 2.0 mL.

[0018] As a preferred technical solution of the present invention, the vacuum drying condition in S5 is 60° C. and the drying time is 1 hour.

[0019] The present invention also provides a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery, wherein the elastic modulus of the hydrogel electrolyte is 0.04-0.05 MPa and the fracture growth rate is 273%.

[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. Improve the mechanical properties and corrosion resistance of the electrolyte: The present invention significantly improves the mechanical properties and corrosion resistance of the electrolyte by introducing polyvinyl alcohol and tetramethyl urea into the hydrogel electrolyte. The low water activity and mechanical strength of polyvinyl alcohol enable the electrolyte material to better resist physical stress and chemical corrosion during use, thereby extending the service life of the battery.

[0021] 2. Improve the ionic conductivity and low temperature performance of the electrolyte: The oxygen-containing groups of tetramethylurea can interact with water molecules, polyvinyl alcohol and zinc ions, regulate the solvation structure of zinc ions, and break the hydrogen bonds between free water molecules. This feature not only improves the ionic conductivity of the electrolyte, but also enables the electrolyte to maintain good performance in low temperature environments, ensuring the normal operation of zinc-ion batteries under cold conditions.

[0022] 3. The preparation method is simple and suitable for large-scale production: The modified hydrogel electrolyte preparation method of the present invention is simple and easy, including steps such as water bath heating dissolution, low temperature freezing and vacuum drying. These steps are simple to operate, easy to control, and do not require complex equipment and expensive materials. They have high production efficiency and cost-effectiveness, and are suitable for large-scale production and practical application promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A diagram showing the foldable hydrogel electrolyte of Example 2; Figure 2 The hydrogen evolution potential diagrams of Example 2 of the present invention and Comparative Examples 1 and 2; Figure 3 The tensile properties of the gel electrolytes obtained in Example 1 and Comparative Example 2 are shown in FIG. Figure 4 The charge and discharge cycle diagram of the zinc battery obtained in Example 2 and Comparative Examples 1 and 2; Figure 5 The room temperature ionic conductivity diagram of Examples 1, 2, 3 and Comparative Example 2.

[0024] Figure 6 This is the low temperature cycle performance diagram of Example 2. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In this embodiment, Figure 1The foldable hydrogel electrolyte of Example 2 is prepared.

[0027] like Figure 2 As shown, it reflects the hydrogen evolution potentials of different gel electrolytes and aqueous electrolytes. The hydrogen evolution potentials of Comparative Example 1, Comparative Example 2, and Example 2 were tested by linear sweep voltammetry. The experimental results show that Example 2 has the highest hydrogen evolution potential.

[0028] like Figure 3 As shown, it reflects the mechanical properties of different gel electrolytes. The tensile properties of Comparative Example 2 and Example 2 were tested by an electronic universal testing machine. The experimental results show that Example 2 has a tensile rate of more than 200%.

[0029] like Figure 4 As shown in the figure, it reflects the different gel electrolytes at 1mAcm -2 The experimental results show that compared with the cycle performance of Comparative Example 2 and Comparative Example 1, Example 2 has the longest cycle time, up to 1000 hours.

[0030] like Figure 5 As shown, it reflects the ionic conductivity of different gel electrolytes. The experimental results show that compared with Comparative Example 2, Example 1 and Example 3, Example 2 has the highest ionic conductivity of 3.97 (H-Siemens / cm).

[0031] like Figure 6 As shown, it reflects the cycle performance of Example 2 at low temperature. Example 2 shows good cycle performance at 0°C for up to more than 400 hours, indicating that it has practical possibility under harsh price adjustment conditions.

[0032] Example 1: Dissolve 7.2706 g of zinc trifluoromethanesulfonate in 10 mL of deionized water. After complete dissolution, add 3 g of polyvinyl alcohol particles to the solution and stir at 90 °C until completely dissolved. Finally, add 0.5 mL of tetramethyl urea and stir until the hydrogel becomes transparent. Place the prepared hydrogel electrolyte in a −15 °C refrigerator and freeze it for more than 12 h, then take it out and thaw it at room temperature. Finally, pour the thawed hydrogel into a mold and dry it at 60 °C for 1 h to remove excess moisture to obtain the fully molded hydrogel electrolyte of Example 1.

[0033] Example 2: Dissolve 7.2706 g of zinc trifluoromethanesulfonate in 10 mL of deionized water. After complete dissolution, add 3 g of polyvinyl alcohol particles to the solution and stir at 90°C until completely dissolved. Finally, add 1 mL of tetramethyl urea and stir until the hydrogel becomes transparent. Place the prepared hydrogel electrolyte in a −15°C refrigerator and freeze it for more than 12 h, then take it out and thaw it at room temperature. Finally, pour the thawed hydrogel into a mold and dry it at 60°C for 1 hour to remove excess moisture to obtain the fully molded hydrogel electrolyte of Example 2.

[0034] Example 3: Dissolve 7.2706 g of zinc trifluoromethanesulfonate in 10 mL of deionized water. After complete dissolution, add 3 g of polyvinyl alcohol particles to the solution and stir at 90°C until completely dissolved. Finally, add 2 mL of tetramethyl urea and stir until the hydrogel becomes transparent. Place the prepared hydrogel electrolyte in a −15°C refrigerator and freeze it for more than 12 h, then take it out and thaw it at room temperature. Finally, pour the thawed hydrogel into a mold and dry it at 60°C for 1 hour to remove excess moisture to obtain the fully molded hydrogel electrolyte of Example 3.

[0035] Comparative Example 1: 7.2706 g of zinc trifluoromethanesulfonate was dissolved in 10 mL of deionized water. After the zinc trifluoromethanesulfonate was completely dissolved, a 2 mol / L liquid electrolyte was obtained.

[0036] Comparative Example 2: Dissolve 7.2706 g of zinc trifluoromethanesulfonate in 10 mL of deionized water. After complete dissolution, add 3 g of polyvinyl alcohol particles to the solution and stir at 90°C until completely dissolved. Place the prepared hydrogel electrolyte in a −15°C refrigerator and freeze for more than 12 h, then take it out and thaw it at room temperature. Finally, pour the thawed hydrogel into the mold and dry it at 60°C for 1 h to remove excess water to obtain a fully shaped hydrogel electrolyte for Comparative Example 2.

[0037] Table 1 Content table of examples and comparative examples Group Polyvinyl alcohol Tetramethylurea Zinc trifluoromethanesulfonate Deionized water Loop duration Example 1 3 g 0.5 mL 7.2706 g 10 mL 180 h Example 2 3 g 1.0 mL 7.2706 g 10 mL 1000 h Example 3 3 g 2.0 mL 7.2706 g 10 mL 230 h Comparative Example 1 0 g 0 mL 7.2706 g 10 mL 70 h Comparative Example 2 3 g 0 mL 7.2706 g 10 mL 100 h The modified hydrogel electrolyte of the present invention uses polyvinyl alcohol as the matrix of the hydrogel and tetramethyl urea as the functional additive, and has excellent mechanical properties. At the same time, the Zn anode is well compatible with the modified hydrogel electrolyte of the present invention. -2 / 1 mA h cm -2 Under the condition of , the Zn||Zn symmetric battery has a stable cycle performance of 1000 h. At the same time, at low temperature, the Zn||Zn battery in Example 2 still has good long cycle performance, which shows the practicality of the modified hydrogel electrolyte of the present invention at low temperature.

[0038] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery, It is characterized in that The following steps are involved: S1: providing a corresponding aqueous solution of zinc trifluoromethanesulfonate; S2: dissolving the polyvinyl alcohol particles by heating and stirring the zinc salt aqueous solution in a water bath; S3: adding tetramethyl urea in different ratios to the polyvinyl alcohol hydrogel electrolyte prepared in S2, and obtaining a uniformly mixed viscous solution by heating and stirring; S4: freezing the obtained viscous solution at low temperature for more than 12 hours; S5: The obtained electrolyte is taken out, cooled to room temperature, and then vacuum dried to obtain a functional hydrogel electrolyte.

2. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The volume ratio of tetramethylurea to water in S3 is 1:20, 1:10, and 1:5; The amount of polyvinyl alcohol is 3 g, and the concentration of zinc trifluoromethanesulfonate is 2 mol / L.

3. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The conditions for water bath heating and stirring in S2 are 80-90° C. and a rotation speed of 100-500 r / min.

4. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The low temperature condition in S4 is -15°C.

5. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The degree of polymerization of the polyvinyl alcohol is 1750±50, and the degree of alcoholysis is 98%±1%.

6. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The dissolution time of the polyvinyl alcohol particles in S2 is 5 to 10 hours.

7. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The added amount of the tetramethyl urea in S3 is 0.5 mL, 1.0 mL, and 2.0 mL.

8. A method for preparing a modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 1, It is characterized in that The vacuum drying condition in S5 is 60° C. and the drying time is 1 hour.

9. A modified hydrogel electrolyte for a quasi-solid-state zinc ion battery, prepared according to the preparation method according to any one of claims 1 to 10.

10. A modified hydrogel electrolyte for a quasi-solid-state zinc ion battery according to claim 9, It is characterized in that The elastic modulus of the hydrogel electrolyte is 0.04~0.05Mpa, and the fracture growth rate is 273%.

Citation Information

Patent Citations

  • Zinc ion battery with self-charging characteristic and preparation method thereof

    CN114551845A

  • Polyvinyl alcohol-based hydrogel electrolyte and preparation method thereof

    CN115172904A

  • Preparation and application of carboxylated cellulose-based flexible zinc dendrite-resistant hydrogel electrolyte

    CN116284855A