Preparation method of ferroelectric polymer film with high piezoelectric coefficient
By adding triethylamine and dehydrochlorination reaction to form P(VDF-TrFE-CFE-FA) tetrapolymer in the preparation of ferroelectric polymer film, and performing spin coating film formation and annealing treatment, the problem of low ferroelectric polymer materials was solved. Regarding electromechanical performance issues, the high-voltage electrical coefficient and electromechanical coupling coefficient have been significantly improved, and are suitable for a variety of application fields.
Patent Information
- Application Number
- CN202410907304.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
AI Technical Summary
The low electromechanical properties of ferroelectric polymer materials limit their performance and practicality in fields such as energy harvesting, imaging, fault detection, ship navigation, and artificial muscles in robots. In particular, their piezoelectric coefficients and electromechanical coupling coefficients are much smaller than those of iron. Electric ceramics.
By stirring P(VDF-TrFE-CFE) terpolymer in N,N-dimethylformamide and adding triethylamine for dehydrochlorination reaction, P(VDF-TrFE-CFE-FA) tetrapolymer is formed. The material is then spin-coated into a film and dried and annealed to prepare a ferroelectric polymer film with high piezoelectric coefficient.
The piezoelectric coefficient d33 and the electromechanical coupling coefficient K of the ferroelectric polymer film are significantly improved, and can achieve a higher piezoelectric effect under a lower electric field, even exceeding the performance of piezoelectric ceramics.
Smart Images

Figure BDA0004932511410000071 
Figure BDA0004932511410000081 
Figure BDA0004932511410000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferroelectric polymers, and more specifically relates to a method for preparing a ferroelectric polymer film with a high piezoelectric coefficient. Background Art
[0002] Currently, ferroelectric polymer materials have been widely used in energy harvesting, acoustic transducers for imaging, fault detection, ship navigation, and artificial muscles in robots. However, the low electromechanical (EM) properties of polymers compared to inorganic materials (piezoelectric ceramics) severely limit their performance and practicality in these applications. The piezoelectric coefficient of the most attractive ferroelectric polymer on the market, polyvinylidene fluoride (PVDF), is only -35pm / V, and the electromechanical coupling coefficient k 33 Only 23%, much smaller than the currently widely used ferroelectric ceramic Pb (TiZr) O3 (PZT), the electromechanical coupling coefficient k of this piezoelectric ceramic is 33 >70%, piezoelectric coefficient d 33 >700pm / V. Meanwhile, although the P(VDF-TrFE-CFE) ternary polymer can achieve a larger electric brake (Dx / DE>400pm / V), this effect is obtained near the breakdown voltage and has no practical application prospects.
[0003] The piezoelectric effect refers to the phenomenon that the piezoelectric body is polarized by external mechanical force, and bound charges with opposite signs appear on the surfaces of both ends of the piezoelectric body. The charge density is proportional to the external mechanical force. This phenomenon is called the positive piezoelectric effect. The piezoelectric body is deformed by the external electric field, and the deformation is proportional to the strength of the external electric field. This phenomenon is called the inverse piezoelectric effect. The positive piezoelectric effect and the inverse piezoelectric effect are collectively called the piezoelectric effect. The piezoelectric coefficient d 33 Used to describe the piezoelectric properties of piezoelectric materials. The larger the piezoelectric coefficient, the better the piezoelectric properties of the material.
[0004] As for polyvinylidene fluoride polymer, it has α, β, γ and other conformations. Among them, the β conformation is the all-trans conformation. Because its atoms are arranged regularly on both sides, it has the largest dipole moment. Therefore, the piezoelectric performance exhibited by the β conformation is the best, and the piezoelectric coefficient d 33 It is also the largest, so in order to improve the piezoelectric properties of polyvinylidene fluoride-based materials, the β conformation should be obtained as much as possible. Summary of the invention
[0005] The present invention aims to provide a method for preparing a ferroelectric polymer film with a high piezoelectric coefficient. The obtained P(VDF-TrFE-CFE-FA) tetrapolymer product contains FA, and the formation of double bonds can reduce the energy required for the polymer to transform into the all-trans conformation β phase. Therefore, the polymer containing double bonds can achieve a better piezoelectric effect under a lower electric field and obtain a higher piezoelectric coefficient d 33 .
[0006] In order to achieve the above object, the present invention is implemented by the following technical scheme: a method for preparing a ferroelectric polymer film with a high piezoelectric coefficient, comprising the following steps:
[0007] (1) P(VDF-TrFE-CFE) terpolymer is added to N,N-dimethylformamide and stirred, and then triethylamine is added to carry out dehydrochlorination to obtain P(VDF-TrFE-CFE-FA) tetrapolymer product;
[0008] (2) The tetramer product is added to N, N-dimethylformamide and stirred, and the obtained polymer solution is spin-coated to form a film, which is then dried and annealed in sequence to obtain a ferroelectric polymer film.
[0009] Further preferably, the ratio of the added amount of the P(VDF-TrFE-CFE) terpolymer to N,N-dimethylformamide is 0.5 g:10-15 mL.
[0010] Further preferably, the ratio of the added amount of the P(VDF-TrFE-CFE) terpolymer to triethylamine is 0.5 g:1 mL.
[0011] Further preferably, the dehydrochlorination process is to place the reaction solution in an oil bath at 50-60° C. and stir the reaction for 20-150 min.
[0012] Further preferably, after the dehydrochlorination process is completed, the solution is poured into an ethanol aqueous solution to collect the precipitate, and the precipitate is dissolved in N,N-dimethylformamide, and the process is repeated 2-3 times. The finally collected precipitate is vacuum dried to obtain a tetramer product.
[0013] Further preferably, the ratio of the added amount of the tetramer product to that of N,N-dimethylformamide is 0.2-0.4 g:5 mL.
[0014] Further preferably, the parameters of the spin coating film formation are: rotation speed 250-350 rpm, rotation time 20-40 s, acceleration 50-60 r / s.
[0015] More preferably, 0.5-1.0 mL of the obtained polymer solution is spin-coated to form a film with a film thickness of 10-15 μm.
[0016] More preferably, the drying is performed at 60-70° C. for 12-24 hours.
[0017] Further preferably, the annealing is performed in a vacuum oven at 120° C. for 24-36 hours with a vacuum degree of 0.1-0.3 MPa.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] (1) Compared with most piezoelectric polymer films on the market at present, the piezoelectric coefficient of the prepared film is 33 The electromechanical coupling coefficient K has been significantly improved, even exceeding that of piezoelectric ceramics.
[0020] (2) The prepared film can obtain a large piezoelectric coefficient under a low electric field of 40-60MV / m. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the infrared spectrum of the tetramer product obtained in Example 4. DETAILED DESCRIPTION
[0022] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0023] Example 1
[0024] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0025] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 30 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0026] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0027] Example 2
[0028] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0029] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 60 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0030] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0031] Example 3
[0032] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0033] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 90 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0034] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0035] Example 4
[0036] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0037] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA), and stir for 120 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1), and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1), and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0038] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0039] Example 5
[0040] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0041] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA), and stir for 150 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0042] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0043] Example 6
[0044] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0045] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 60 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0046] (2) Dissolve 0.4 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 1.0 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 200 rpm, a rotation time of 30 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0047] Example 7
[0048] A ferroelectric polymer film with a high piezoelectric coefficient is prepared as follows:
[0049] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA), and stir for 120 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1), and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1), and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0050] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 h, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 130°C for 24 h with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0051] Comparative Example 1: Preparation of P(VDF-TrFE-CFE) terpolymer film
[0052] (1) 0.3 g of P(VDF-TrFE-CFE) trimer powder was dissolved in 5 ml of DMF solution and stirred overnight.
[0053] (2) The spin coater was set to a rotation speed of 250 r, a rotation time of 20 s, and an acceleration of 50 r / s. 0.8 mL of the obtained polymer solution was dropped onto a clean glass substrate to form a film by spin coating.
[0054] (3) The film was placed in an oven at 60°C and dried for 12 h. The film was then soaked in clean water and peeled off the glass plate.
[0055] (4) Finally, the film was annealed in a vacuum oven at 120°C for 24 h with a vacuum degree of 0.1 MPa to obtain the final terpolymer film.
[0056] Comparative Example 2: Compared with Example 1, no annealing was performed.
[0057] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 30 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0058] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 h, soak it in clean water, and peel the film off the glass plate. Finally, dry the film in an oven at 60°C for 6 h to obtain the final ferroelectric polymer film.
[0059] Comparative Example 3: Compared with Example 1, the annealing time is too short.
[0060] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 30 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0061] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of N,N-dimethylformamide and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 hours, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 12 hours with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0062] Comparative Example 4: Compared with Example 1, the film-forming solution used is DMSO solution.
[0063] (1) Dissolve 0.5 g of P(VDF-TrFE-CFE) terpolymer in 10 mL of N,N-dimethylformamide and stir overnight. Then place the solution in an oil bath at 50°C, add 1 mL of triethylamine (TEA) and stir for 30 min. Then pour the reaction solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. Redissolve the precipitate in 15 mL of N,N-dimethylformamide, stir evenly, and then pour the solution into a mixed solution of 200 mL of water and ethanol (volume ratio of 1:1) and collect the precipitate. The collected precipitate is placed in a vacuum oven at 45°C and dried for 24 h to obtain the final tetramer product.
[0064] (2) Dissolve 0.3 g of the tetramer product powder in 5 mL of DMSO and stir overnight. Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and spin coat it into a film. The spin coater is set to a speed of 250 rpm, a rotation time of 20 s, an acceleration of 50 r / s, and a spin-coated film thickness of 12 μm. Then dry it in an oven at 60°C for 12 h, soak it in clean water, and peel the film off the glass plate. Finally, anneal the film in a vacuum oven at 120°C for 24 h with a vacuum degree of 0.1 MPa to obtain the final ferroelectric polymer film.
[0065] Table 1
[0066]
[0067]
[0068] As shown in Table 1, Examples 1-5 show that the FA content increases with the increase of reaction time, and the best piezoelectricity is shown when the reaction time is 120 min and the FA content is 1.9%. Example 5 has more FA content than Example 4 but shows lower piezoelectric performance. This is because when the double bond content exceeds 1.9%, the negative impact of the double bonds on the structure and performance of the material will be further increased. Too many double bonds will increase the rigidity of the polymer chain, limit the mobility of the chain segments, make it difficult for the dipoles to be redirected under the electric field, and lead to lower d 33 ; Too many double bonds will significantly reduce the crystallinity of the material and make the amorphous region too large. Although the amorphous region helps polarization, too many amorphous regions will reduce the mechanical properties of the material, thereby reducing its piezoelectric properties; a high content of double bonds may introduce more structural defects, which will lead to uneven material properties and thus reduce the overall piezoelectric coefficient.
[0069] Although embodiment 6 has the same double bond content compared to embodiment 1, it shows lower piezoelectric performance, because the concentration of solution can affect the solubility of polymer in solvent, interchain interaction and final film-forming process.When 0.3g product is dissolved in 5mL DMF, the concentration is moderate (about 0.06g / mL), which can ensure that polymer chain is fully launched and evenly dispersed in solution.Moderate concentration helps to form uniform film in subsequent film-forming process, avoids the aggregation or uneven distribution of polymer chain, so as to obtain ideal microstructure.When the polymer solution concentration is too high, high concentration can cause the interaction between polymer chains to increase, and chain entanglement and aggregation phenomenon are obvious, causing solution viscosity to increase, the film formed is uneven, and internal defects increase.It may cause phase separation in film-forming process, forming uneven microstructure, affecting piezoelectric performance.When high concentration solution is in film-forming, solvent volatilization is uneven, which may cause residual solvent or hole in the film, affecting the mechanical and electrical properties of material. When the concentration of the polymer solution is too low, the low concentration will cause the polymer chains to be sparsely distributed in the solution, and the formed film may be incomplete, insufficiently thick, and have poor mechanical strength and uniformity. At low concentrations, the interaction between polymer chains is weakened, which may lead to unsatisfactory chain arrangement and crystallinity, affecting the polarization process and piezoelectric properties. Excessive solvent will evaporate during the film formation process, which may cause shrinkage and holes in the film, affecting the performance of the material.
[0070] Compared with Example 4, Example 7 has the same FA content, but exhibits lower piezoelectric performance. This is because the annealing process changes the microstructure of the polymer through heat treatment, including crystallinity, grain size and internal stress, which in turn affects its performance. The annealing temperature of 120°C is an optimized temperature, which makes the crystallinity of the polymer reach an optimal balance point, with sufficient crystalline areas to provide mechanical strength and polarization response, and an appropriate amount of amorphous areas to enable the dipole moment to be redirected under the electric field. Annealing makes the grain size moderate, and smaller grains have more grain boundaries, which contribute to the polarization process to a certain extent and improve the piezoelectric performance. The annealing temperature of the degree helps to release the stress inside the material, reduce defects and cracks, and improve the stability of the piezoelectric performance. When the annealing temperature is too high: high temperature may cause excessive crystallization of the polymer, resulting in a reduction in amorphous areas. Although high crystallinity contributes to the mechanical strength of the material, too few amorphous areas make it difficult to redirect the dipole moment and reduce the piezoelectric coefficient. High temperature will cause excessive growth of grains, reduce grain boundaries, and reduce the polarization ability of the material. Too high a temperature may also cause thermal degradation of the polymer, destroying the molecular chain structure and further reducing the performance. When the annealing temperature is too low: the polymer is not fully crystallized at low temperatures, the crystalline area is not sufficient to provide sufficient mechanical strength and polarization response, and the piezoelectric coefficient will decrease. Low-temperature annealing is not enough to effectively release the stress inside the material, and there may be more internal defects and stress concentration, affecting the piezoelectric performance. Low-temperature annealing may lead to uneven grain size distribution, further affecting the piezoelectric performance. Ultimately, 120°C annealing provides a moderate degree of crystallinity and a balanced microstructure, which allows the polarity and mechanical properties inside the material to achieve the best balance, thereby obtaining the best piezoelectric coefficient d 33 .
[0071] like Figure 1As shown, it can also be seen from the infrared spectrum that the reaction product P(VDF-TrFE-CFE-FA) has a slight increase in the β phase of the all-trans conformation and a corresponding decrease in the α phase compared with the raw material P(VDF-TrFE-CFE). The molecular chain arrangement in the all-trans conformation is relatively linear, which makes the electric dipoles on the chain segments arranged in the same direction, making polarization easier to achieve. The crystal region formed by the all-trans conformation has higher mechanical and electrical stability, and can more effectively transfer external stress to the internal electric dipoles, thereby increasing the piezoelectric modulus. Annealing can release the residual stress inside the polymer, allowing the chain segments to have more degrees of freedom to rearrange and tend to the all-trans conformation. In addition, the chain segments of the all-trans conformation are arranged uniformly and orderly, reducing the structural defects inside the material and improving the piezoelectric performance. During the annealing process, the chain segments gradually arrange into an all-trans conformation with a more consistent polarization direction. This consistency improves the response of the material under an electric field, making the piezoelectric effect more significant. This makes it easier for the molecular chains to rearrange under the electric field, improving the polarization efficiency and enabling the material to convert mechanical energy and electrical energy more efficiently. Ultimately, annealing promotes the crystallization and orderly arrangement of the polymer by increasing the all-trans conformation, releasing internal stress and improving the consistency of the polarization direction. These factors work together to enhance the polarization and piezoelectric response of the material, thereby improving the piezoelectric performance. Therefore, the more all-trans conformation β, the larger the piezoelectric coefficient and the better the piezoelectric performance.
[0072] Table 2
[0073]
[0074] As shown in Table 2, the piezoelectric coefficients of Comparative Example 1 and Example 4 were measured and counted, where the comparative example is the highest piezoelectric coefficient that can be achieved. For PVDF-based materials, when mechanical stress is applied, the electric dipoles inside the material will be rearranged, thereby generating charges. This rearrangement causes the direction of charge generation to be opposite to the direction of the applied stress, so it is manifested as a negative piezoelectric coefficient. Example 4 polarized and measured the piezoelectric coefficient under low electric fields of 20MV / m, 30MV / m, and 40MV / m, respectively, and compared with Comparative Example 1, Comparative Example 1 needs to reach a piezoelectric coefficient of 400pm / V under a high electric field of 100MV / m, which is the data obtained near the breakdown voltage of Comparative Example 1. Such a high voltage will not be allowed in actual production applications, thus severely limiting its application. The electric field required for Example 4 is much smaller than that of Comparative Example 1, and the piezoelectric performance is also very excellent. Finally, it can be seen that the piezoelectric performance of the relevant ferroelectric polymer film can be significantly improved by the method of this patent, and exceeds the piezoelectric coefficient of piezoelectric ceramics widely used on the market. It shows broad application prospects and markets.
[0075] Table 3
[0076]
[0077] As shown in Table 3, the piezoelectric coefficients of Example 1 and Comparative Examples 2-4 under an electric field of 40 MV / m were measured and statistically analyzed, among which Example 1 exhibited the best piezoelectric coefficient.
[0078] Example 1 has a higher piezoelectric coefficient than Comparative Example 2 and Comparative Example 3, because in the unannealed polymer material, the molecular segments are usually in a disordered or partially ordered state. This disordered state can lead to inconsistent polarization directions, so that the electric dipoles cannot be effectively arranged, the polarization efficiency is low, and the piezoelectric performance is poor. The crystallinity of the unannealed material is usually low, and there is a lack of sufficient ordered crystal regions. The lack of crystal regions means that the material cannot effectively transfer stress and charge under the action of an electric field or stress, resulting in a decrease in piezoelectric performance. There may be more residual stress in the unannealed material, which will hinder the movement and rearrangement of the molecular segments, reduce the polarization efficiency and piezoelectric response. At the same time, the annealing time is too short to provide enough thermal energy to allow the polymer segments to obtain sufficient movement and rearrangement opportunities. The segments remain in a disordered or partially ordered state, and the polarization efficiency is not high. The annealing time is not enough to allow the polymer segments to fully form stable crystal regions. Some crystal regions may not have been fully developed, resulting in low crystallinity of the material and inability to fully improve the piezoelectric performance. The annealing time is too short and may not be enough to release all internal residual stresses. These stresses will continue to exist, affecting the arrangement and polarization process of molecular segments and reducing the piezoelectric performance.
[0079] Example 1 has a higher piezoelectric coefficient than Comparative Example 4. This is because although DMSO has a larger dipole moment than DMF, it is not suitable for the preparation of tetramer films, and the uniformity of the film will deteriorate and the piezoelectric performance will be unsatisfactory.
[0080] The above embodiments of the present invention are merely examples for illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all the embodiments here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a ferroelectric polymer film with a high piezoelectric coefficient, characterized in that: The steps include: (1) P(VDF-TrFE-CFE) terpolymer is added to N,N-dimethylformamide and stirred, and then triethylamine is added to dehydrochlorinate to obtain a tetramer product; (2) The tetramer product is added to N, N-dimethylformamide and stirred, and the obtained polymer solution is spin-coated to form a film, which is then dried and annealed in sequence to obtain a ferroelectric polymer film.
2. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, characterized in that: The ratio of the added amount of the P(VDF-TrFE-CFE) terpolymer to that of N,N-dimethylformamide is 0.5 g:10-15 mL.
3. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, characterized in that: The ratio of the added amount of the P(VDF-TrFE-CFE) terpolymer to triethylamine is 0.5 g:1 mL.
4. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in any one of claims 1 to 3, characterized in that: The dehydrochlorination process is to place the reaction solution in an oil bath at 50-60°C and stir the reaction for 20-150 minutes.
5. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 4, characterized in that: After the dehydrochlorination process is completed, the solution is poured into an ethanol aqueous solution to collect the precipitate, and the precipitate is dissolved in N, N-dimethylformamide, and the process is repeated 2-3 times. The finally collected precipitate is vacuum dried to obtain a tetramer product.
6. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, characterized in that: The ratio of the added amount of the tetramer product to that of N,N-dimethylformamide is 0.2-0.4 g:5 mL.
7. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, characterized in that: The parameters of the spin coating film formation are: rotation speed 250-350 rpm, rotation time 20-40 s, acceleration 50-60 r / s.
8. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, 6 or 7, characterized in that: 0.5-1.0 mL of the obtained polymer solution was spin-coated to form a film with a film thickness of 10-15 μm.
9. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1, characterized in that: The drying is carried out at 60-70° C. for 12-24 hours.
10. The method for preparing a ferroelectric polymer film with a high piezoelectric coefficient as claimed in claim 1 or 9, characterized in that: The annealing is carried out in a vacuum oven at 120° C. for 24-36 hours with a vacuum degree of 0.1-0.3 MPa.
Citation Information
Cited By
Synthetic method for improving acoustoelectric conversion response of polyvinylidene fluoride-based polymer and application of synthetic method
CN119912621A
Chiral P (VDF-TrFE-CFE)-based quaternary block ferroelectric polymer material and preparation method thereof
CN120944006A
A chiral p(vdf-trfe-cfe) based quaternary ferroelectric polymer material and a method of making the same
CN120944006B
Grafted ferroelectric polymer film with high piezoelectric coefficient and preparation method thereof
CN121159905A
A ferroelectric polymer thin film with high piezoelectric coefficient and a preparation method thereof
CN121159905B