Patterned proton exchange membrane and preparation method and application thereof
By setting a patterned structure on the surface of the proton exchange membrane, the problem of smooth and dense existing membrane surfaces is solved, forming a three-dimensional structure, increasing the contact area between the catalytic layer and the membrane, and significantly improving the performance and stability of the fuel cell.
Patent Information
- Application Number
- CN202410833260.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-15
AI Technical Summary
The surface of existing commercial proton exchange membranes is smooth and dense, resulting in poor interface structure between the catalytic layer and the membrane, which affects the performance of the fuel cell.
Patterned structures are set on the surface of the proton exchange membrane, including groove, spiral or lattice patterns with a depth of 0.5 μm to 100 μm, and are coated with resin to enhance the contact area between the catalytic layer and the membrane.
By forming a three-dimensional structure, the contact area between the catalytic layer and the proton membrane is significantly increased, the interface structure is improved, and the performance and stability of the fuel cell are improved, including improved mechanical properties and electrochemical properties.
Smart Images

Figure CN118782847A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ion batteries, and in particular relates to a patterned proton exchange membrane and a preparation method and application thereof. Background Art
[0002] Compared with traditional energy conversion technologies such as internal combustion engines, fuel cells are a highly efficient energy conversion device that converts chemical energy in fuels (such as hydrogen, methanol, ethanol or natural gas) into electrical energy. The reaction process is not limited by the Carnot cycle and has higher energy conversion efficiency and lower greenhouse gas emissions. It is widely used in automobiles and portable power devices.
[0003] Among many fuel cells, proton exchange membrane fuel cells are considered to be the most promising energy conversion device due to their cleanliness, high efficiency, zero pollution, low operating temperature, and rapid startup. As a key component of proton exchange membrane fuel cells, proton exchange membrane (PEM) is mainly responsible for transmitting protons and blocking fuel penetration. Its performance directly determines the service life and efficiency of proton exchange membrane fuel cells.
[0004] In order to obtain a more efficient, safe and durable proton exchange membrane fuel cell, the proton exchange membrane should have the following advantages: 1) High proton conductivity. Proton conductivity is one of the most critical properties of PEM. Fast and efficient proton transfer is bound to obtain excellent PEMFC performance. Under normal conditions, the proton conductivity can reach the order of 0.1S / cm. 2) Good resistance to gas permeation. Low gas permeation is an important basis for PEMFC to maintain long-term operation. If the gas permeation is serious, a part of the open circuit voltage will be lost, resulting in a decrease in the output performance of PEMFC. 3) Good chemical stability. The proton exchange membrane material with a stable chemical structure will degrade slowly when running in the fuel cell. 4) High mechanical stability. When the proton exchange membrane is assembled into a membrane electrode, the tensile strength must be ≥5MPa, otherwise the membrane material is easily crushed and causes a loss of battery performance. 5) Excellent thermal stability. The proton exchange membrane material has good thermal stability, so that the contact between the membrane material and the catalyst will not be poor due to thermal degradation.
[0005] However, the existing commercial proton exchange membrane is mainly perfluorosulfonic acid proton membrane. If we seek a breakthrough in the pure material system, it is difficult to further improve the performance of fuel cells. In addition, the proton membrane produced by the current commercial proton membrane preparation process usually has a smooth and dense surface, which is close to a two-dimensional plane, and there is a poor interface structure between its surface and the catalyst layer. Summary of the invention
[0006] The embodiments of the present invention provide a patterned proton exchange membrane and a preparation method and application thereof, aiming to solve the problems that the existing commercial proton exchange membrane has a smooth and dense surface and a poor interface structure between the surface and the catalytic layer.
[0007] In order to achieve the above-mentioned purpose, on the one hand, an embodiment of the present invention provides a patterned proton exchange membrane, including a membrane body, wherein a plurality of patterns are evenly arranged on the side of the membrane body close to the catalytic layer, and the catalytic layer is adapted to the pattern; the depth of the pattern is 0.5μm to 100μm; and the surface of the pattern is coated with resin.
[0008] As a preferred embodiment, the pattern is at least one of a groove pattern, a spiral pattern or a dot pattern.
[0009] As a preferred embodiment, when the pattern is a gully pattern, the depth of the gully pattern is 0.5 μm to 100 μm, and the width is 0.5 μm to 100 μm; and the spacing between adjacent gully patterns is 0.5 μm to 100 μm.
[0010] As a preferred embodiment, the membrane body is an expanded porous membrane, preferably an ePTFE membrane.
[0011] On the other hand, an embodiment of the present invention further provides a method for preparing the patterned proton exchange membrane, comprising the following steps:
[0012] S01, coating a first resin on the side of a plate to obtain a coated plate; the side is provided with a plurality of patterns; the coating height is 10 μm to 240 μm;
[0013] S02, laying the expanded porous film flat on the coated surface of the coated plate to obtain a flat plate; drying the flat plate to obtain a dried plate;
[0014] S03, coating the second resin on the expanded porous film surface of the dried plate, drying it once and then drying it twice to obtain a patterned proton exchange membrane; the coating height is 10 μm to 240 μm.
[0015] As a preferred embodiment, in step S01,
[0016] The first resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone, preferably short side branched perfluorosulfonic acid.
[0017] The plate is one of plastic, stainless steel, acrylic, glass, PTFE, PEEK or ceramic, or a mixture of at least two of them.
[0018] The pattern is at least one of a gully pattern, a spiral pattern or a dot pattern.
[0019] The pattern is obtained by laser engraving, CNC milling or 3D printing.
[0020] The coating height is preferably 180 μm.
[0021] As a preferred embodiment, in step S02,
[0022] The expanded porous film is one of expanded porous polytetrafluoroethylene, expanded porous polybenzimidazole, expanded porous polyethylene, expanded porous polystyrene, artificial graphite or expanded porous polyethyleneimine, or a mixture of at least two of them.
[0023] The expanded porous film is fixed and stretched by a frame to achieve flat laying; the frame is a plastic frame, a stainless steel frame, an acrylic frame or a glass frame.
[0024] The drying temperature is 40° C. to 80° C., preferably 50° C. to 70° C.; the drying time is 5 min to 60 min, preferably 10 min to 40 min.
[0025] The drying is achieved by using an air drying oven.
[0026] As a preferred embodiment, in step S03,
[0027] The second resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone, preferably short side branched perfluorosulfonic acid.
[0028] The temperature of the primary drying is 40° C. to 80° C., preferably 50° C. to 70° C.; the time of the primary drying is 5 min to 60 min, preferably 10 min to 40 min.
[0029] The temperature of the secondary drying is 100° C. to 200° C., preferably 110° C. to 190° C.; the time of the secondary drying is 30 min to 300 min, preferably 60 min to 240 min.
[0030] The primary drying and the secondary drying are achieved by using an air blast drying box.
[0031] The coating height is preferably 180 μm.
[0032] On the other hand, an embodiment of the present invention further provides an application of the patterned proton exchange membrane, wherein the patterned proton exchange membrane is applied in a fuel cell.
[0033] Compared with the prior art, the present application has the following technical effects: by setting a pattern on the surface of the proton membrane, the surface of the proton membrane can be constructed from a two-dimensional plane to a three-dimensional structure, which can greatly increase the contact area between the catalyst layer and the proton membrane, thereby effectively improving the interface structure, forming more effective three-phase interfaces, and promoting efficient mass transfer between different components, thereby improving the performance of the fuel cell. The patterned proton exchange membrane of the present application has good stability and excellent mechanical and electrochemical properties. It can be used in fuel cells to effectively improve the mass transfer problem in the membrane electrode and significantly improve the polarization performance of the fuel cell. The preparation method of the present application is simple, easy to operate, low in cost, short in preparation time, and easy to realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0035] Figure 1 It is a schematic diagram of the cross-sectional structure after the catalytic layer of the patterned proton exchange membrane according to one embodiment of the present application is combined with the proton exchange membrane. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0038] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0039] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0040] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0041] In the present application, by setting a pattern on the surface of the proton membrane and controlling the relevant parameters of the pattern (such as depth, width and spacing, etc.), the surface of the proton membrane can be constructed from a two-dimensional plane into a three-dimensional structure, which can greatly increase the contact area between the catalyst layer and the proton membrane, thereby effectively improving the interface structure, forming more effective three-phase interfaces, promoting efficient mass transfer between different components, and thereby improving the performance of the fuel cell.
[0042] On the one hand, an embodiment of the present invention provides a patterned proton exchange membrane, including a membrane body, wherein a plurality of patterns are evenly arranged on the side of the membrane body close to the catalytic layer, and the catalytic layer is adapted to the pattern; the depth of the pattern is 0.5μm to 100μm (depending on the actual use needs, it can be 0.5μm, or 15μm, or 30μm, or 60μm, or 100μm, etc.); the surface of the pattern is coated with resin.
[0043] As a preferred embodiment, the pattern is at least one of a groove pattern, a spiral pattern or a dot pattern.
[0044] As a preferred embodiment, when the pattern is a groove type pattern, the depth of the groove type pattern is 0.5μm to 100μm (depending on the actual use needs, it can be 0.5μm, or 10μm, or 30μm, or 60μm, or 100μm, etc.), and the width is 0.5μm to 100μm (depending on the actual use needs, it can be 0.5μm, or 15μm, or 30μm, or 75μm, or 100μm, etc.); the spacing between adjacent groove type patterns is 0.5μm to 100μm (depending on the actual use needs, it can be 0.5μm, or 15μm, or 35μm, or 70μm, or 100μm, etc.).
[0045] The specific shape of the pattern can be selected according to actual use needs. Specifically, in this embodiment, Figure 1 As shown, the pattern is a gully pattern. The depth of the gully pattern is 3 μm, the width is 2 μm, and the spacing between adjacent gully patterns is 2 μm.
[0046] As a preferred embodiment, the membrane body is an expanded porous membrane, preferably an ePTFE membrane.
[0047] On the other hand, an embodiment of the present invention further provides a method for preparing the patterned proton exchange membrane, comprising the following steps:
[0048] S01, coating the first resin on the side of the plate to obtain a coated plate; the side is provided with a plurality of patterns; the coating height is 10 μm to 240 μm (depending on the actual use requirements, it can be 10 μm, or 50 μm, or 150 μm, or 240 μm, etc.);
[0049] S02, laying the expanded porous film flat on the coated surface of the coated plate to obtain a flat plate; drying the flat plate to obtain a dried plate;
[0050] S03. Coating a second resin on the expanded porous film surface of the dried plate, drying it once and then drying it twice to obtain a patterned proton exchange membrane; the coating height is 10μm to 240μm (depending on the actual needs, it can be 10μm, or 50μm, or 150μm, or 240μm, etc.).
[0051] As a preferred embodiment, in step S01,
[0052] The first resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone, preferably short side branched perfluorosulfonic acid.
[0053] The plate is one of plastic, stainless steel, acrylic, glass, PTFE, PEEK or ceramic, or a mixture of at least two of them.
[0054] The pattern is at least one of a gully pattern, a spiral pattern or a dot pattern.
[0055] The pattern is obtained by laser engraving, CNC milling or 3D printing.
[0056] The coating height is preferably 180 μm.
[0057] As a preferred embodiment, in step S02,
[0058] The expanded porous film is one of expanded porous polytetrafluoroethylene, expanded porous polybenzimidazole, expanded porous polyethylene, expanded porous polystyrene, artificial graphite or expanded porous polyethyleneimine, or a mixture of at least two of them.
[0059] The expanded porous film is fixed and stretched by a frame to achieve flat laying; the frame is a plastic frame, a stainless steel frame, an acrylic frame or a glass frame.
[0060] The drying temperature is 40°C to 80°C (depending on the actual needs, it can be 40°C, 50°C, 70°C, 80°C, etc.); the drying time is 5min to 60min (depending on the actual needs, it can be 5min, 10min, 25min, 60min, etc.).
[0061] The drying is achieved by using an air drying oven.
[0062] As a preferred embodiment, in step S03,
[0063] The second resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone, preferably short side branched perfluorosulfonic acid.
[0064] The temperature of the primary drying is 40°C to 80°C (depending on the actual needs, it can be 40°C, 50°C, 70°C, 80°C, etc.); the time of the primary drying is 5min to 60min (depending on the actual needs, it can be 5min, 10min, 25min, 60min, etc.).
[0065] The temperature of the secondary drying is 100°C to 200°C (depending on the actual needs, it can be 100°C, or 110°C, or 150°C, or 200°C, etc.); the time of the secondary drying is 30min to 300min (depending on the actual needs, it can be 30min, or 60min, or 240min, or 300min, etc.).
[0066] The primary drying and the secondary drying are achieved by using an air blast drying box.
[0067] The coating height is preferably 180 μm.
[0068] Specifically, in one embodiment, the method for preparing the patterned proton exchange membrane comprises the following steps:
[0069] S01, coating a first resin on the side of a plate to obtain a coated plate; the side is provided with a plurality of patterns; the coating height is 200 μm;
[0070] S02, laying the expanded porous film flat on the coated surface of the coated plate to obtain a flat plate; drying the flat plate to obtain a dried plate;
[0071] S03, coating the second resin on the expanded porous film surface of the dried plate, drying it once and then drying it twice to obtain a patterned proton exchange membrane; the coating height is 200 μm.
[0072] In step S01,
[0073] The first resin is short-side branched perfluorosulfonic acid.
[0074] The plate is glass.
[0075] like Figure 1 As shown, the pattern is a gully pattern, the depth of the gully pattern is 3 μm, the width is 2 μm, and the spacing between adjacent gully patterns is 2 μm.
[0076] The pattern is obtained by laser engraving.
[0077] In step S02,
[0078] The expanded porous film is an ePTFE film.
[0079] The expanded porous film is fixed and stretched by a frame to achieve flat laying; the frame is a plastic frame.
[0080] The drying temperature is 60° C. and the drying time is 30 min.
[0081] The drying is achieved by using an air drying oven.
[0082] In step S03,
[0083] The second resin is a short-side branched perfluorosulfonic acid.
[0084] The temperature of the first drying is 60° C.; the time of the first drying is 30 minutes.
[0085] The temperature of the secondary drying is 150° C.; the time of the secondary drying is 30 minutes.
[0086] The primary drying and the secondary drying are achieved by using an air blast drying box.
[0087] The thickness of the prepared patterned proton exchange membrane is 25 microns, the tensile strength is 51 MPa, and the elongation at break is 141%. At 80°C and 50% relative humidity, the proton conductivity is 121 mS / cm; the hydrogen permeability is 0.025 mL / min·cm 2 The patterned proton exchange membrane was installed in a single cell for testing, and the membrane electrode impedance was 2.1mΩ and the polarization performance was 0.662V@2A / cm 2 It can be seen that the prepared patterned proton exchange membrane meets the relevant requirements of fuel cell proton exchange membrane.
[0088] Comparative Example 1
[0089] A method for preparing a proton exchange membrane comprises the following steps:
[0090] S01, coating the first resin on the side of the plate to obtain a coated plate; the coating height is 200 μm;
[0091] S02, laying the expanded porous film flat on the coated surface of the coated plate to obtain a flat plate; drying the flat plate to obtain a dried plate;
[0092] S03, coating the second resin on the expanded porous film surface of the dried plate, drying it once and then drying it twice to obtain a proton exchange membrane; the coating height is 200 μm.
[0093] In step S01,
[0094] The first resin is short-side branched perfluorosulfonic acid.
[0095] The plate is glass.
[0096] In step S02,
[0097] The expanded porous film is an ePTFE film.
[0098] The expanded porous film is fixed and stretched by a frame to achieve flat laying; the frame is a plastic frame.
[0099] The drying temperature is 60° C. and the drying time is 30 min.
[0100] The drying is achieved by using an air drying oven.
[0101] In step S03,
[0102] The second resin is a short-side branched perfluorosulfonic acid.
[0103] The temperature of the first drying is 60° C.; the time of the first drying is 30 minutes.
[0104] The temperature of the secondary drying is 150° C.; the time of the secondary drying is 30 minutes.
[0105] The primary drying and the secondary drying are achieved by using an air blast drying box.
[0106] The thickness of the prepared proton exchange membrane is 23 microns, the tensile strength is 48 MPa, and the elongation at break is 131%. At 80°C and 50% relative humidity, the proton conductivity is 111 mS / cm; the hydrogen permeability is 0.026 mL / min·cm 2 The proton exchange membrane was installed in a single cell for testing, and the membrane electrode impedance was 3.2mΩ and the polarization performance was 0.641V@2A / cm 2 .
[0107] In the description of this specification, the description with reference to the terms "an embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0108] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A patterned proton exchange membrane, It is characterized in that It comprises a membrane body, wherein a plurality of patterns are evenly arranged on the side of the membrane body close to the catalytic layer, and the catalytic layer is arranged to match the patterns; the depth of the patterns is 0.5 μm to 100 μm; and the surface of the patterns is coated with resin.
2. The patterned proton exchange membrane according to claim 1, It is characterized in that The pattern is at least one of a gully pattern, a spiral pattern or a dot pattern.
3. The patterned proton exchange membrane according to claim 2, It is characterized in that When the pattern is a gully pattern, the depth of the gully pattern is 0.5 μm to 100 μm, and the width is 0.5 μm to 100 μm; the interval between adjacent gully patterns is 0.5 μm to 100 μm.
4. The patterned proton exchange membrane according to claim 1, It is characterized in that The membrane body is an expanded porous membrane.
5. The method for preparing a patterned proton exchange membrane according to any one of claims 1 to 4, It is characterized in that The steps include: S01, coating a first resin on the side of a plate to obtain a coated plate; the side is provided with a plurality of patterns; the coating height is 10 μm to 240 μm; S02, laying the expanded porous film flat on the coated surface of the coated plate to obtain a flat plate; drying the flat plate to obtain a dried plate; S03, coating the second resin on the expanded porous film surface of the dried plate, drying it once and then drying it twice to obtain a patterned proton exchange membrane; the coating height is 10 μm to 240 μm.
6. The method for preparing the patterned proton exchange membrane according to claim 5, It is characterized in that In step S01, The first resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone; The plate is one of plastic, stainless steel, acrylic, glass, PTFE, PEEK or ceramic, or a mixture of at least two of them; The pattern is at least one of a gully pattern, a spiral pattern or a dot pattern; The pattern is obtained by laser engraving, CNC milling or 3D printing.
7. The method for preparing the patterned proton exchange membrane according to claim 5, It is characterized in that In step S02, The expanded porous film is one or a mixture of at least two of expanded porous polytetrafluoroethylene, expanded porous polybenzimidazole, expanded porous polyethylene, expanded porous polystyrene, artificial graphite or expanded porous polyethyleneimine; The drying temperature is 40° C. to 80° C.; the drying time is 5 min to 60 min.
8. The method for preparing the patterned proton exchange membrane according to claim 5, It is characterized in that In step S03, The second resin is one or a mixture of at least two of phenolic resin, epoxy resin, polyimide, polyvinylidene fluoride, short side branched perfluorosulfonic acid, polyvinylidene fluoride, benzoxazine, liquid crystal resin, asphalt, polyphenylene sulfide, polyetheretherketone, epoxy resin and polyethersulfone; The temperature of the primary drying is 40° C. to 80° C.; the time of the primary drying is 5 min to 60 min.
9. The method for preparing the patterned proton exchange membrane according to claim 5, It is characterized in that In step S03, The temperature of the secondary drying is 100°C to 200°C; the time of the secondary drying is 30min to 300min; The primary drying and the secondary drying are achieved by using an air blast drying box.
10. Use of the patterned proton exchange membrane according to any one of claims 1 to 4, It is characterized in that The patterned proton exchange membrane is applied in a fuel cell.