Method and system for preparing electrolyte by coupling ammonium polyvanadate

The all-vanadium redox flow battery electrolyte is prepared by the ammonium polyvanadate pyrolysis reduction method, and the residual ammonia decomposition system and the waste heat utilization system are used to solve the problems of complex electrolyte preparation process and non-environmental protection in the existing technology, and achieve high efficiency and low cost. Cost-effective, environmentally friendly electrolyte preparation and battery performance improvement.

CN118782850APending Publication Date: 2024-10-15NANJING WONDUX ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410914128.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing all-vanadium redox flow battery electrolyte preparation process is complex, high-cost, and not environmentally friendly. In particular, a large amount of harmful gases and wastewater are generated during the electrolyte preparation process, which affects environmental protection.

Method used

Ammonium polyvanadate is used as raw material, the electrolyte is prepared by pyrolysis reduction method, and the hydrogen generated by the residual ammonia decomposition system is used as the reducing agent to realize the reduction reaction in a closed environment, and the heat utilization rate is improved through the waste heat utilization system, and a mixed acid system is used Increase the vanadium content in the electrolyte and add an optimization agent to improve the stability of the electrolyte.

Benefits of technology

The electrolyte preparation process is simplified, the cost is reduced, the green and environmentally friendly electrolyte preparation is achieved, and the vanadium content of the electrolyte is improved and the performance of the all-vanadium redox flow battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The method comprises the following steps: feeding an ammonium polyvanadate mixture into a pyrolysis reduction furnace, carrying out a pyrolysis coupling reduction reaction in an inert atmosphere, decomposing residual ammonia to generate hydrogen, providing a reducing agent for the pyrolysis coupling reduction reaction, and preparing a vanadium oxide with an average valence state of 3.5, the method comprises the following steps: dissolving vanadium oxide with an average valence state of 3.5 in ultrapure water and a mixed acid solution to form a 3.5-valence mixed acid electrolyte; and the 3.5-valence mixed acid electrolyte is cleaned and optimized to obtain the qualified electrolyte. According to the method, ammonia gas generated by pyrolysis of ammonium polyvanadate is coupled with hydrogen generated by decomposition of redundant ammonia gas to serve as a reducing agent, compared with other additional reducing agents, the cost of the reducing agent is greatly reduced, and therefore the preparation cost of the vanadium battery electrolyte is reduced, meanwhile, no harmful gas is generated and discharged in the whole technological process, and the method is suitable for industrial production. The electrolyte is green and environment-friendly in preparation and low in cost, and continuous large-scale production can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an electrolyte by coupling ammonium polyvanadate and a system thereof, relates to the preparation of an electrolyte for an all-vanadium liquid flow battery, and belongs to the field of vanadium electrolyte preparation. Background Art

[0002] At present, the technological development and application of renewable energy have made important breakthroughs internationally. The development speed of new renewable energy such as wind energy and solar energy is the fastest, showing the strong vitality of renewable energy as the dominant energy in the 21st century. However, whether it is the use of wind energy or solar energy, it requires excellent energy storage devices to match it, which can play the role of storage when there is surplus electricity and power supply when there is a shortage of electricity. Energy storage technology is mainly divided into electrochemical energy storage and physical energy storage. According to the research report of the International Electrochemical Energy Storage Technology Association (ESA), the ideal form for large-scale fixed energy storage is still the liquid flow energy storage system. Among them, all-vanadium liquid flow battery is a hot topic of concern. The electrolyte is the energy storage medium of the all-vanadium liquid flow battery and the key material of the all-vanadium liquid flow battery. The performance of the electrolyte directly determines the energy storage capacity of the liquid flow battery, and the cost of the electrolyte significantly affects the industrialization of its liquid flow battery.

[0003] Most of the existing patents use V2O5 or ammonium metavanadate as raw materials to prepare electrolytes by chemical methods or electrolytic methods. Patent (CN 114156497 A) uses calcium carbonate as a catalyst, separates and purifies the obtained ore powder multiple times to obtain ammonium metavanadate, and then purifies the crude ammonium metavanadate solution to obtain a high-purity ammonium metavanadate solution, and then dehydrates the ammonium metavanadate to obtain ammonium metavanadate powder. The ammonium metavanadate powder is washed with ammonium chloride solution to obtain vanadium pentoxide powder, and the vanadium pentoxide powder is mixed with concentrated sulfuric acid and sulfur to obtain vanadium sulfate (III), and vanadium sulfate (III) is decomposed to obtain vanadium sulfate, and finally the vanadium sulfate is mixed with dilute sulfuric acid to obtain vanadium sulfate electrolyte. Patent (CN 114275811 A) first calcines and reduces the crude vanadium compound to convert it into VO 2+ or vanadium sulfate VOSO4, and then add acid to dissolve the reduced calcined product into vanadium sulfate or vanadium dichloride solution, use an organic extractant to extract vanadium, and obtain VO 2+ The solution containing VO 2+The solution is electrolytically reduced to obtain a vanadium electrolyte with an average valence of 3.5. Patent (CN 103401010 A): V2O5 powder is reduced to V2O4 powder and V2O3 powder in a hydrogen atmosphere, and the reduced V2O4 powder is dissolved in concentrated sulfuric acid to obtain a tetravalent vanadium sulfate solution for use as the positive electrode electrolyte of the vanadium battery, and the reduced V2O3 powder is dissolved in concentrated sulfuric acid to obtain a divalent vanadium sulfate solution for use as the negative electrode electrolyte of the vanadium battery, or the reduced V2O4 powder and V2O3 powder are evaporated and crystallized in 6-18.4 mol / L sulfuric acid to obtain VOSO4 and V2(SO4)3 crystals, and the VOSO4 and V2(SO4)3 crystals are dissolved in dilute sulfuric acid to obtain a vanadium electrolyte for all-vanadium liquid flow batteries. Patent (CN 115411326 A): Provide an aqueous solution of ammonium metavanadate, use the aqueous solution of ammonium metavanadate as a cathode liquid, use a sulfuric acid solution as an anode liquid, perform a first-stage electrolysis in an electrolysis device, filter the obtained cathode liquid, add a sulfuric acid solution to the cathode tank, perform a second-stage electrolysis, and obtain a vanadium electrolyte in the cathode tank.

[0004] Among the various methods mentioned above, vanadium pentoxide or ammonium metavanadate is mostly used as raw materials, and the electrolyte is prepared by chemical reduction acid dissolution or electrolysis. The patent (CN 114156497 A) has a long process flow, the preparation of the electrolyte is complicated, and a large amount of ammonium-containing wastewater will be generated during the production process, which is not environmentally friendly. The patent (CN 114275811 A) uses an extraction method to produce a large amount of oil-containing wastewater and waste gas, which is not green and environmentally friendly. The patent (CN 103401010 A) uses hydrogen reduction, and does not mention the source of hydrogen and the use of reduction heat. The current cost of hydrogen reduction is relatively high. The patent (CN 115411326 A) produces a large amount of ammonia during electrolysis of ammonium metavanadate. If the ammonia is not handled properly, it will cause environmental problems. The electrolyte preparation process of the above method is complicated, a large amount of harmful gases are generated during the preparation of the electrolyte, which is not green and environmentally friendly, and the comprehensive cost of preparing the electrolyte is high; a single acid is used as a supporting liquid, and the vanadium content of the electrolyte is not high. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a method and system for preparing an electrolyte by coupling ammonium polyvanadate in view of the shortcomings of the prior art.

[0006] To solve the above problems, the present invention adopts the following solution: A method for preparing an electrolyte by coupling ammonium polyvanadate, characterized in that it comprises the following steps: Step 1: feeding the ammonium polyvanadate mixture into a pyrolysis reduction furnace, sealing the pyrolysis reduction furnace and filling it with an inert protective gas, sequentially performing drying preheating, pyrolysis reaction, and reduction reaction in the pyrolysis reduction furnace, and further thermally cracking part of the ammonia generated by the pyrolysis of the ammonium polyvanadate mixture to generate initial hydrogen as a reducing agent to participate in the reduction reaction; Step 2: The ammonia that fails to participate in the reduction reaction is sent to the residual ammonia decomposition system to decompose the ammonia into nitrogen and hydrogen, of which part of the hydrogen is supplemented into the pyrolysis reduction furnace as a reducing agent, and the other part is used as a heat source for the pyrolysis reduction furnace, part of the nitrogen is used as an inert protective gas, and the rest is stored as a by-product; Step 3: by adjusting the amount of reducing agent added, the residence time of the ammonium polyvanadate mixture in the pyrolysis reduction furnace, the reduction reaction temperature, and the reduction depth, the molar amount of V2O4 substance in the low-valent vanadium oxide product of the pyrolysis reduction furnace: the molar amount of V2O3 substance = (0.948-1.052): (0.948-1.052), that is, the average valence of vanadium is 3.5; Step 4: injecting low-valent vanadium oxide and ultrapure water into a dissolution tank, stirring while injecting, and then adding a mixed acid of sulfuric acid and hydrochloric acid; finally obtaining an electrolyte having a 3.5-valent electrolyte vanadium concentration of 1.5-2.5 mol / L, a sulfate concentration of 2.0-3.0 mol / L, and a chloride ion concentration of 5.9-6.5 mol / L; The ammonium polyvanadate reducing agent is hydrogen produced by the thermal decomposition of ammonium polyvanadate to produce ammonia coupled with the residual ammonia decomposition system; the excess coefficient of the ammonium polyvanadate reducing agent is 1.2 to 1.35.

[0007] Furthermore, the method for preparing an electrolyte by coupling ammonium polyvanadate is characterized in that, in step 1, the ammonium polyvanadate mixture needs to be screened before being fed into a pyrolysis reduction furnace, and the screening accuracy is 100-130 meshes.

[0008] Furthermore, the method for preparing electrolyte by coupling ammonium polyvanadate is characterized in that the high-temperature gas discharged from the outer cylinder of the pyrolysis reduction furnace is recovered through a waste heat utilization system, and the inlet air sent to the combustion aid of the pyrolysis reduction furnace is preheated.

[0009] Furthermore, the method for preparing an electrolyte by coupling ammonium polyvanadate is characterized in that the pyrolysis reduction furnace is divided into a retort section, a pyrolysis section, and a reduction section; the temperature of the retort section of the pyrolysis reduction furnace is controlled at 150°C to 200°C, the residence time of the retort section is controlled at 0.5h to 1h, the temperature of the pyrolysis section is controlled at 450°C to 500°C, the residence time of the pyrolysis section is controlled at 1h to 1.5h, the temperature of the reduction section is controlled at 550°C to 600°C, and the residence time of the reduction section is controlled at 1.5h to 2h; the pressure of the pyrolysis reduction furnace is controlled at -50Pa to 500Pa.

[0010] Furthermore, the method for preparing an electrolyte by coupling ammonium polyvanadate is characterized in that the electrolyte in step four is sent to a membrane filter for filtration, and an electrolyte optimizer is added to the filtrate; the electrolyte optimizer is one or more of sodium sulfate, glycerol, dilute phosphoric acid solution, NaHSO4, K2SO4 and KHSO4, wherein the amount of sodium sulfate and glycerol added is not higher than 2%; the amount of dilute phosphoric acid solution added is less than 3%; the amount of NaHSO4, K2SO4 and KHSO4 added is about 1%.

[0011] An ammonium polyvanadate coupled electrolyte preparation method and an ammonium polyvanadate coupled electrolyte preparation system, characterized in that it comprises an ammonium polyvanadate pretreatment and transportation system, an ammonium polyvanadate thermal decomposition coupled reduction system, a residual ammonia decomposition system, a residual heat utilization system, and an electrolyte preparation system; The ammonium polyvanadate pretreatment and delivery system is connected to the ammonium polyvanadate thermal decomposition coupled reduction system, and is used to screen the ammonium polyvanadate mixture and deliver it to the ammonium polyvanadate thermal decomposition coupled reduction system; The ammonium polyvanadate thermal decomposition coupled reduction system prepares vanadium oxide with an average valence of 3.5 through thermal decomposition coupled reduction; The excess ammonia decomposition system is connected to the exhaust port of the ammonium polyvanadate pyrolysis coupled reduction system; it is used to decompose the ammonia-containing gas generated by the pyrolysis reduction of the ammonium polyvanadate mixture into nitrogen and hydrogen, the hydrogen is returned to the ammonium polyvanadate pyrolysis reduction system as a reducing agent and fuel, and the nitrogen is used as a byproduct; The preheating and utilization system is connected to the high-temperature gas outlet of the ammonium polyvanadate thermal decomposition coupled reduction system to recover waste heat from the high-temperature gas discharged from the ammonium polyvanadate thermal decomposition coupled reduction system for preheating the air inlet of the combustion aid of the ammonium polyvanadate thermal decomposition coupled reduction system; The electrolyte preparation system is connected to the discharge port of the ammonium polyvanadate thermal decomposition coupled reduction system, and is used to configure the discharged low-valent vanadium oxide with an average valence of 3.5 into an electrolyte, and perform filtering optimization.

[0012] Furthermore, the ammonium polyvanadate coupled electrolyte preparation system is characterized by comprising an ammonium polyvanadate pretreatment and transportation system, an ammonium polyvanadate thermal decomposition coupled reduction system, a residual ammonia decomposition system, a residual heat utilization system, and an electrolyte preparation system; The ammonium polyvanadate pretreatment conveying system comprises a vibrating screen, a receiving hopper, a Z-shaped conveyor, a feeding hopper, and a feeding machine; a receiving hopper is arranged at the bottom of the vibrating screen, a discharge port of the receiving hopper is connected to a feeding port of the Z-shaped conveyor, a discharge port of the Z-shaped conveyor is connected to a feeding port of the feeding hopper, a discharge port of the feeding hopper is connected to a feeding port of the feeding machine, and a discharge port of the feeding machine is connected to a feeding port of the ammonium polyvanadate thermal decomposition coupled reduction system; The ammonium polyvanadate pyrolysis coupled reduction system comprises a pyrolysis reduction furnace, a combustion aid, and a cooling conveyor; a combustion aid is provided at the bottom of the outer cylinder of the pyrolysis reduction furnace to provide heat to the pyrolysis reduction furnace, the feed inlet of the pyrolysis reduction furnace is connected to the outlet of the feeder, the discharge port of the pyrolysis reduction furnace is connected to the feed inlet of the cooling conveyor, the high-temperature gas outlet of the outer cylinder of the pyrolysis reduction furnace is connected to the inlet of the combustion-supporting air heat exchanger, and the reduction gas outlet of the pyrolysis reduction furnace is connected to the air inlet of the rectifier dust collector; The residual ammonia decomposition system comprises a rectifier dust collector, an ammonia decomposition reactor, a heat exchanger, a dryer, a fan, a gas membrane separation device, a hydrogen storage tank, and a nitrogen storage tank; the air inlet of the rectifier dust collector is connected to the reducing gas exhaust port of the pyrolysis reduction furnace, the outlet of the rectifier dust collector is connected to the inlet of the ammonia decomposition reactor, the outlet of the ammonia decomposition reactor is connected to the air inlet of the heat exchanger, the exhaust port of the heat exchanger is connected to the inlet of the dryer, the outlet of the dryer is connected to the inlet of the fan, the outlet of the fan is connected to the air inlet of the gas membrane separation device, the hydrogen exhaust port of the gas membrane separation device is connected to the air inlet of the hydrogen storage tank, and the nitrogen exhaust port of the gas membrane separation device is connected to the air inlet of the nitrogen storage tank; the hydrogen storage tank is connected to the reducing agent addition port of the pyrolysis reduction furnace and the fuel gas addition port of the combustion aid, and controllers are respectively provided to adjust the reducing agent addition amount and the heating temperature; The waste heat utilization system includes a combustion-supporting air heat exchanger, an induced draft fan, an exhaust pipe, and a combustion-supporting air fan; the hot gas inlet of the combustion-supporting air heat exchanger is connected to the exhaust port of the outer cylinder of the pyrolysis reduction furnace, the hot gas outlet of the combustion-supporting air heat exchanger is connected to the air inlet of the induced draft fan, the cold air outlet of the combustion-supporting air heat exchanger is connected to the combustion-supporting air of the combustion-supporting furnace, the cold air inlet of the combustion-supporting air heat exchanger is connected to the outlet of the combustion-supporting air fan, and the air outlet of the induced draft fan is connected to the inlet of the exhaust pipe; the high-temperature gas discharged from the outer cylinder of the pyrolysis reduction furnace is used to heat the combustion-supporting air entering the combustion-supporting furnace; The electrolyte preparation system includes a dissolution tank, a filter pump, a membrane filter, and an electrolyte optimization tank; the dissolution tank feed port is connected to the cooling conveyor discharge port, the dissolution tank discharge port is connected to the filter pump inlet, the filter pump outlet is connected to the membrane filter water inlet, the membrane filter water outlet is connected to the electrolyte optimization tank feed port, and the membrane filter concentrate outlet is connected to the dissolution tank circulating water outlet.

[0013] Furthermore, the ammonium polyvanadate coupling electrolyte preparation system is characterized in that the vibrating screen is a single-layer linear vibrating screen with a vibrating screen accuracy of 100 to 130 meshes; the feed hopper is designed with an anti-bridging agitator, a cycloidal precision feeder is arranged between the feed hopper and the feeder, and a material seal plus nitrogen sealing is arranged at the same time; the feeder is a single-axis flexible spiral, and a 15 cm to 20 cm material seal section is provided at the discharge end.

[0014] Furthermore, the ammonium polyvanadate coupling electrolyte preparation system is characterized in that the pyrolysis reduction furnace is a quantum furnace, the inner cylinder is made of stainless steel, and the pyrolysis reduction furnace is divided into a retort section, a pyrolysis section, and a reduction section; the temperature of each section is accurately controlled by the power and number of the combustion aids set in each section; a combustion aid is set at every 1.3m to 1.5m in the retort section of the pyrolysis reduction furnace, a combustion aid is set at every 1.0m to 1.2m in the pyrolysis section of the pyrolysis reduction furnace, and a combustion aid is set at every 0.7m to 0.9m in the reduction section of the pyrolysis reduction furnace.

[0015] Furthermore, the ammonium polyvanadate coupling electrolyte preparation system is characterized in that the rectifier dust collector is of ceramic filter element type, and is provided with nitrogen regular purge and automatic ash removal device; the gas membrane separation device adopts hollow fiber membrane, and after separation, the hydrogen purity is 92% to 98%, and the nitrogen purity is 96% to 99.9%.

[0016] Furthermore, the ammonium polyvanadate coupled electrolyte preparation system is characterized in that the combustion-supporting air heat exchanger is made of stainless steel, the high-temperature gas temperature entering the combustion-supporting air heat exchanger is 450°C to 500°C, the gas temperature exiting the combustion-supporting air heat exchanger is 200°C to 220°C, the combustion air temperature entering the combustion-supporting air heat exchanger is normal temperature, and the combustion air temperature exiting the combustion-supporting air heat exchanger is 180°C to 200°C.

[0017] Furthermore, the ammonium polyvanadate coupling electrolyte preparation system is characterized in that the membrane filter is a ceramic membrane or a silicon carbide membrane, the membrane is in the form of a flat membrane or a cylindrical mold, and the accuracy of the membrane is not less than 60μm.

[0018] The design scheme of the present invention includes an ammonium polyvanadate pretreatment and transportation system, an ammonium polyvanadate thermal decomposition coupled reduction system, a residual ammonia decomposition system, a residual heat utilization system, and an electrolyte preparation system. The method uses high-purity ammonium polyvanadate as a raw material, and prepares vanadium oxide with an average valence of 3.5 by thermal decomposition coupled reduction. The vanadium oxide with an average valence of 3.5 is dissolved in ultrapure water and a mixed acid solution to form a 3.5-valent mixed acid electrolyte. The 3.5-valent mixed acid electrolyte is cleaned and optimized to obtain a qualified electrolyte, which can be directly used in an all-vanadium liquid flow battery stack. The ammonia-containing gas generated by the thermal decomposition reduction of ammonium polyvanadate enters an ammonia decomposition furnace and is decomposed into nitrogen and hydrogen. The hydrogen returns to the ammonium polyvanadate thermal decomposition reduction system as a reducing agent and fuel, and the nitrogen is a by-product. The gas after heat exchange with the heat source is used to recover its heat for residual heat.

[0019] The technical effects of the present invention are as follows: it overcomes the problems that the electrolyte preparation can only use vanadium pentoxide and ammonium metavanadate as raw materials, the electrolyte preparation process is long, the electrolyte preparation cost is high, the electrolyte preparation process is not environmentally friendly, and the vanadium content of the electrolyte is not high.

[0020] (1) The electrolyte was prepared by using ammonium polyvanadate as raw material through reduction and acid dissolution, which broadened the raw materials for preparing the electrolyte of all-vanadium liquid flow battery.

[0021] (2) The use of a quantum furnace to pyrolyze and reduce ammonium polyvanadate can achieve precise control, good pyrolysis and reduction effects, high heat utilization, and greatly reduce operating costs.

[0022] (3) Self-produced hydrogen is used as fuel to provide the required heat for the thermal decomposition reduction of ammonium polyvanadate. The entire heating process does not produce any harmful gases, which is green and environmentally friendly.

[0023] (4) Ammonium polyvanadate is pyrolyzed to produce ammonia and reducing gas, which is then coupled to hydrogen produced by an ammonia decomposition device. The entire reduction process is carried out in a closed environment without leakage and without the need to add additional reducing agent. The pyrolysis reducing gas produced produces hydrogen and nitrogen after passing through the ammonia decomposition device. The hydrogen is used internally and the nitrogen is sold externally. There is no gas discharge during the entire process, and the sale of by-product nitrogen has certain economic benefits, which effectively reduces operating costs.

[0024] (5) The vanadium content in the electrolyte was increased by using a mixed acid system, and the stability of the electrolyte was improved by adding an optimizer, thereby improving the performance of the all-vanadium liquid flow battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the process of preparing electrolyte by coupling ammonium polyvanadate.

[0026] Among them: 1. Vibrating screen; 2. Receiving hopper; 3. Z-type conveyor; 4. Feed hopper; 5. Feeder; 6. Pyrolysis reduction furnace; 7. Combustion aid; 8. Cooling conveyor; 9. Combustion-supporting air heat exchanger; 10. Induced draft fan; 11. Exhaust pipe; 12. Combustion-supporting fan; 13. Rectifier dust collector; 14. Ammonia decomposition reactor; 15. Heat exchanger; 16. Dryer; 17. Fan; 18. Gas membrane separation device; 19. Hydrogen storage tank; 20. Nitrogen storage tank; 21. Dissolution tank; 22. Filter pump; 23. Membrane filter; 24. Electrolyte optimization tank; 25. Ammonium polyvanadate pretreatment and transportation system; 26. Ammonium polyvanadate pyrolysis coupled reduction system; 27. Residual ammonia decomposition system; 28. Residual heat utilization system; 29. ​​Electrolyte preparation system. DETAILED DESCRIPTION

[0027] The following is a detailed description of this patent in conjunction with the accompanying drawings and implementation cases. It is understood that the specific implementation cases described here are only used to explain the relevant patent content, rather than to limit the patent. It should also be noted that for the sake of ease of description, only the parts related to the patent are illustrated in the accompanying drawings.

[0028] like Figure 1As shown, a preferred implementation case of the present patent provides an ammonium polyvanadate coupled electrolyte preparation system and method, the system comprising an ammonium polyvanadate pretreatment and transportation system 25, an ammonium polyvanadate thermal decomposition coupled reduction system 26, a residual ammonia decomposition system 27, a waste heat utilization system 28, and an electrolyte preparation system 29.

[0029] After the high-purity ammonium polyvanadate raw material is unpacked, it is poured onto the vibrating screen 1. The materials that meet the particle size requirements of the vibrating screen 1 fall into the receiving hopper 2, and the materials that do not meet the particle size requirements are selected by the vibrating screen 1. The selected materials are processed and then screened by the vibrating screen 1. The screening accuracy of the vibrating screen 1 is 100-130 meshes. The purpose of screening is to prevent large pieces of materials from entering the system and being pyrolyzed and reduced incompletely. The materials in the receiving hopper 2 fall onto the belt of the receiving port of the Z-type conveyor 3 through the chute. The Z-type conveyor 3 sends the materials to the discharge port through the belt movement and falls into the feed hopper 4. The Z-type conveyor 3 is a folded-edge fully sealed type. The materials in the feed hopper 4 are accurately and evenly fed into the feeder 5 through the cycloidal precision feeder at the bottom. The feed hopper 4 is provided with an anti-bridge agitator, the feed hopper 4 is conical, and is also provided with a nitrogen filling pipeline, which is sealed with nitrogen to isolate the air. The feeder 5 is a single-axis flexible spiral, and a 15cm-20cm material sealing section is provided at the discharge end.

[0030] The feeder 5 uniformly and quantitatively delivers the material to the inner cylinder of the pyrolysis reduction furnace 6. The material is heated in the pyrolysis reduction furnace 6 to undergo pyrolysis reduction reaction, reducing the high-valent vanadium into 4-valent and 3-valent vanadium oxides. After pyrolysis reduction, the material enters the cooling conveyor 8, which cools the material to 100°C to 150°C and then discharges it into the dissolution tank 21. The pyrolysis reduction furnace 6 is a quantum furnace, which is divided into a dry distillation section, a pyrolysis section, and a reduction section; the temperature of the dry distillation section is controlled at 150°C to 200°C, the residence time of the dry distillation section is controlled at 0.5h to 1h, the temperature of the pyrolysis section is controlled at 450°C to 500°C, the residence time of the pyrolysis section is controlled at 1h to 1.5h, the temperature of the reduction section is controlled at 550°C to 600°C, and the residence time of the reduction section is controlled at 1.5h to 2h; the pressure of the pyrolysis reduction furnace 6 is controlled at -50Pa to 500Pa. The ammonium polyvanadate reducing agent is the hydrogen generated by the coupling of ammonia produced by the pyrolysis of ammonium polyvanadate and the reduction gas to the residual ammonia decomposition system 27. After the material reduction is completed, a sample is taken from the outlet of the cooling conveyor 8 to analyze the valence of vanadium. The uniform valence of vanadium is 3.5 and is considered qualified. The heat source of the pyrolysis reduction furnace 6 is the hydrogen generated by the residual ammonia decomposition system 27. The high-temperature gas generated by the combustion of hydrogen in the pyrolysis reduction furnace 6 is sent to the residual heat utilization system 28 for residual heat utilization after heat exchange. The pyrolysis reduction gas of the pyrolysis reduction furnace 6 is sent to the residual ammonia decomposition system 27 for recycling.

[0031] The high-temperature gas from the pyrolysis reduction 6 first passes through the combustion air heat exchanger 9 under the action of the induced draft fan 10, and the high-temperature gas temperature is reduced to a safe temperature, and then safely discharged through the exhaust pipe 11. The temperature of the high-temperature gas entering the combustion air heat exchanger 9 is 450℃~500℃, and the temperature of the gas leaving the combustion air heat exchanger 9 is 200℃~220℃. The temperature of the combustion air entering the combustion air heat exchanger 9 is normal temperature, and the temperature of the combustion air leaving the combustion air heat exchanger 9 is 180℃~200℃. The combustion air sent to the combustion air heat exchanger 9 by the combustion air fan 12 is used as the air supply for the combustion air 7 of the pyrolysis reduction furnace 9 after heat exchange.

[0032] The pyrolysis reduction gas of the pyrolysis reduction furnace 6 first passes through the rectifying dust collector 13 to remove dust, and after dust removal, the clean high-temperature pyrolysis reduction gas enters the ammonia decomposition reactor 14; the clean high-temperature pyrolysis reduction gas contains a certain amount of ammonia and hydrogen, and the clean high-temperature pyrolysis reduction gas undergoes a decomposition reaction of ammonia in the ammonia decomposition reactor 14 to generate nitrogen and hydrogen; the nitrogen and hydrogen generated by the ammonia decomposition reactor 14 are cooled by heat exchanger 15 and dehydrated by dryer 16, and then sent to the gas membrane separation device 18 through fan 17; the gas membrane separation device 18 is arranged with a hollow fiber membrane to separate hydrogen and nitrogen, and the hydrogen flows into the hydrogen storage tank 19 for storage and is used by the system, and the nitrogen flows into the nitrogen storage tank 20 for storage and sale. The rectifying dust collector 13 is a ceramic filter element type, and is provided with a nitrogen regular purge and an automatic ash discharge device; the gas membrane separation device 18 uses a hollow fiber membrane, and the purity of hydrogen after separation is 92% to 98%, and the purity of nitrogen is 96% to 99.9%.

[0033] The reduced low-valent vanadium oxide is put into the dissolution tank 21, and the amount of water and acid is set according to the amount of low-valent vanadium oxide added. The operation process is to start the dissolution tank 21 to stir while adding low-valent vanadium oxide and ultrapure water. When the ultrapure water and low-valent vanadium oxide are added, a certain amount of acid is slowly added. The acid added to the dissolution tank is a mixed acid of sulfuric acid and hydrochloric acid. The final electrolyte has a 3.5-valent electrolyte vanadium concentration of 1.5~2.5 mol / L, a sulfate concentration of 2.0~3.0 mol / L, and a chloride ion concentration of 5.9~6.5mol / L. The electrolyte that has reacted completely in the dissolution tank 2 is sent to the membrane filter 23 through the filter pump 22, and the membrane filter 23 filters and removes impurities from the electrolyte. The membrane filter 23 produces water that flows into the electrolyte optimization tank 24, and the electrolyte optimization tank 24 is started to stir and add the electrolyte optimizer. The electrolyte optimizer is one or more of sodium sulfate, glycerol, dilute phosphoric acid solution, NaHSO4, K2SO4 and KHSO4. The amount of sodium sulfate and glycerol added is not more than 2%; the amount of dilute phosphoric acid solution added is less than 3%; the amount of NaHSO4, K2SO4 and KHSO4 added is about 1%. The optimized electrolyte is sampled and analyzed, and canned and sold after passing the test.

Claims

1. A method for preparing an electrolyte by coupling ammonium polyvanadate, characterized in that: The following steps are included: Step 1: feeding the ammonium polyvanadate mixture into a pyrolysis reduction furnace, sealing the pyrolysis reduction furnace and filling it with an inert protective gas, sequentially performing drying, pyrolysis reaction, and reduction reaction in the pyrolysis reduction furnace, and further thermally cracking part of the ammonia generated by the pyrolysis of the ammonium polyvanadate mixture to generate initial hydrogen as a reducing agent to participate in the reduction reaction; Step 2: The ammonia that fails to participate in the reduction reaction is sent to the residual ammonia decomposition system to decompose the ammonia into nitrogen and hydrogen, of which part of the hydrogen is supplemented into the pyrolysis reduction furnace as a reducing agent, and the other part is used as a heat source for the pyrolysis reduction furnace, part of the nitrogen is used as an inert protective gas, and the rest is stored as a by-product; Step 3: by adjusting the amount of reducing agent added, the residence time of the ammonium polyvanadate mixture in the pyrolysis reduction furnace, the reduction reaction temperature, and the reduction depth, the molar amount of V2O4 substance in the low-valent vanadium oxide product of the pyrolysis reduction furnace: the molar amount of V2O3 substance = (0.948-1.052): (0.948-1.052), that is, the average valence of vanadium is 3.5; Step 4: injecting low-valent vanadium oxide and ultrapure water into a dissolution tank, stirring while injecting, and then adding a mixed acid of sulfuric acid and hydrochloric acid; finally obtaining an electrolyte having a 3.5-valent electrolyte vanadium concentration of 1.5-2.5 mol / L, a sulfate concentration of 2.0-3.0 mol / L, and a chloride ion concentration of 5.9-6.5 mol / L; The ammonium polyvanadate reducing agent is hydrogen produced by coupling ammonia produced by thermal decomposition of ammonium polyvanadate with an ammonia decomposition system (27); and the excess coefficient of the ammonium polyvanadate reducing agent is 1.2 to 1.

35.

2. The method for preparing an electrolyte by coupling ammonium polyvanadate according to claim 1, characterized in that: Step 1: The ammonium polyvanadate mixture needs to be screened before being sent into the pyrolysis reduction furnace, and the screening accuracy is 100-130 meshes.

3. The method for preparing an electrolyte by coupling ammonium polyvanadate according to claim 1, characterized in that: The high-temperature gas discharged from the outer cylinder of the pyrolysis reduction furnace is recovered through the waste heat utilization system, and the inlet air sent to the combustion aid of the pyrolysis reduction furnace is preheated.

4. The method for preparing an electrolyte by coupling ammonium polyvanadate according to claim 1, characterized in that: The pyrolysis reduction furnace is divided into a retort section, a pyrolysis section, and a reduction section; the temperature of the retort section of the pyrolysis reduction furnace is controlled at 150°C to 200°C, and the residence time of the retort section is controlled at 0.5h to 1h; the temperature of the pyrolysis section is controlled at 450°C to 500°C, and the residence time of the pyrolysis section is controlled at 1h to 1.5h; the temperature of the reduction section is controlled at 550°C to 600°C, and the residence time of the reduction section is controlled at 1.5h to 2h; the pressure of the pyrolysis reduction furnace (6) is controlled at -50Pa to 500Pa.

5. The method for preparing electrolyte by coupling ammonium polyvanadate according to claim 1, characterized in that: The electrolyte in step 4 is sent to a membrane filter for filtration, and an electrolyte optimizer is added to the filtrate; the electrolyte optimizer is one or more of sodium sulfate, glycerol, dilute phosphoric acid solution, NaHSO4, K2SO4 and KHSO4, wherein the amount of sodium sulfate and glycerol added is not higher than 2%; the amount of dilute phosphoric acid solution added is less than 3%; the amount of NaHSO4, K2SO4 and KHSO4 added is about 1%.

6. An ammonium polyvanadate coupling system for preparing an electrolyte using the method for preparing an electrolyte by ammonium polyvanadate coupling according to claim 1, characterized in that: It includes an ammonium polyvanadate pretreatment and transportation system (25), an ammonium polyvanadate thermal decomposition coupled reduction system (26), a residual ammonia decomposition system (27), a residual heat utilization system (28), and an electrolyte preparation system (29); The ammonium polyvanadate pretreatment and delivery system (25) is connected to the ammonium polyvanadate thermal decomposition coupled reduction system (26) and is used to screen the ammonium polyvanadate mixture and deliver it to the ammonium polyvanadate thermal decomposition coupled reduction system (26); The ammonium polyvanadate thermal decomposition coupled reduction system (26) prepares vanadium oxide with an average valence of 3.5 by thermal decomposition coupled reduction; The excess ammonia decomposition system (27) is connected to the exhaust port of the ammonium polyvanadate thermal decomposition coupled reduction system (26); It is used to decompose the ammonia gas produced by the pyrolysis reduction of the ammonium polyvanadate mixture into nitrogen and hydrogen, the hydrogen is returned to the ammonium polyvanadate pyrolysis reduction system as a reducing agent and fuel, and the nitrogen is a by-product; The preheating and utilization system (28) is connected to the high-temperature gas outlet of the ammonium polyvanadate thermal decomposition coupled reduction system (26) to recover waste heat from the high-temperature gas discharged from the ammonium polyvanadate thermal decomposition coupled reduction system (26) for preheating the air inlet of the combustion aid (7) of the ammonium polyvanadate thermal decomposition coupled reduction system (26); The electrolyte preparation system (29) is connected to the discharge port of the ammonium polyvanadate thermal decomposition coupled reduction system (26) and is used to prepare the discharged low-valent vanadium oxide with an average valence of 3.5 into an electrolyte and perform filtration optimization.

7. The ammonium polyvanadate coupled electrolyte preparation system according to claim 6, characterized in that: It includes an ammonium polyvanadate pretreatment and transportation system (25), an ammonium polyvanadate thermal decomposition coupled reduction system (26), a residual ammonia decomposition system (27), a residual heat utilization system (28), and an electrolyte preparation system (29); The ammonium polyvanadate pretreatment conveying system (25) comprises a vibrating screen (1), a receiving hopper (2), a Z-shaped conveyor (3), a feed hopper (4), and a feed machine (5); a receiving hopper (2) is arranged at the bottom of the vibrating screen (1); the discharge port of the receiving hopper (2) is connected to the feed port of the Z-shaped conveyor (3); the discharge port of the Z-shaped conveyor (3) is connected to the feed port of the feed hopper (4); the discharge port of the feed hopper (4) is connected to the feed port of the feed machine (5); and the discharge port of the feed machine (5) is connected to the feed port of the ammonium polyvanadate thermal decomposition coupled reduction system (26); The ammonium polyvanadate pyrolysis coupled reduction system (26) comprises a pyrolysis reduction furnace (6), a combustion aid (7), and a cooling conveyor (8); a combustion aid (7) is provided at the bottom of the outer cylinder of the pyrolysis reduction furnace (6) to provide heat to the pyrolysis reduction furnace (6); the feed port of the pyrolysis reduction furnace (6) is connected to the outlet of the feed machine (5); the discharge port of the pyrolysis reduction furnace (6) is connected to the feed port of the cooling conveyor (8); the high-temperature gas outlet of the outer cylinder of the pyrolysis reduction furnace (6) is connected to the inlet of the combustion-supporting air heat exchanger (9); and the reduction gas outlet of the pyrolysis reduction furnace (6) is connected to the air inlet of the rectifier dust collector (13); The residual ammonia decomposition system (27) comprises a rectifier dust collector (13), an ammonia decomposition reactor (14), a heat exchanger (15), a dryer (16), a fan (17), a gas membrane separation device (18), a hydrogen storage tank (19), and a nitrogen storage tank (20); the air inlet of the rectifier dust collector (13) is connected to the reducing gas outlet of the pyrolysis reduction furnace (6), the outlet of the rectifier dust collector (13) is connected to the inlet of the ammonia decomposition reactor (14), the outlet of the ammonia decomposition reactor (14) is connected to the air inlet of the heat exchanger (15), and the heat exchanger (15) is connected to the reducing gas outlet of the pyrolysis reduction furnace (6). ) the exhaust port is connected to the inlet of the dryer (16), the outlet of the dryer (16) is connected to the inlet of the fan (17), the outlet of the fan (17) is connected to the air inlet of the air membrane separation device (18), the hydrogen outlet of the air membrane separation device (18) is connected to the air inlet of the hydrogen storage tank (19), and the nitrogen outlet of the air membrane separation device (18) is connected to the air inlet of the nitrogen storage tank (20); the hydrogen storage tank (19) is connected to the reducing agent addition port of the pyrolysis reduction furnace (6) and the fuel gas addition port of the combustion aid (7), and controllers are respectively provided to adjust the reducing agent addition amount and the heating temperature; The waste heat utilization system (28) comprises a combustion-supporting air heat exchanger (9), an induced draft fan (10), an exhaust pipe (11), and a combustion-supporting air fan (12); the hot gas inlet of the combustion-supporting air heat exchanger (9) is connected to the exhaust port of the outer cylinder of the pyrolysis reduction furnace (6), the hot gas outlet of the combustion-supporting air heat exchanger (9) is connected to the air inlet of the induced draft fan (10), the cold gas outlet of the combustion-supporting air heat exchanger (9) is connected to the combustion-supporting air of the combustion aid (7), the cold gas inlet of the combustion-supporting air heat exchanger (9) is connected to the outlet of the combustion-supporting air fan (12), and the air outlet of the induced draft fan (10) is connected to the inlet of the exhaust pipe (11); the high-temperature gas discharged from the outer cylinder of the pyrolysis reduction furnace (6) is used to heat the combustion-supporting air entering the combustion aid (7); The electrolyte preparation system (29) comprises a dissolving tank (21), a filtration pump (22), a membrane filter (23), and an electrolyte optimization tank (24); the feed port of the dissolving tank (21) is connected to the discharge port of the cooling conveyor (8), the discharge port of the dissolving tank (21) is connected to the inlet of the filtration pump (22), the outlet of the filtration pump (22) is connected to the water inlet of the membrane filter (23), the water production port of the membrane filter (23) is connected to the feed port of the electrolyte optimization tank (24), and the concentrated water port of the membrane filter (23) is connected to the circulating water port of the dissolving tank (21).

8. The ammonium polyvanadate coupled electrolyte preparation system according to claim 7, characterized in that: The vibrating screen (1) is a single-layer linear vibrating screen, and the accuracy of the vibrating screen (1) is 100 to 130 meshes; the feed hopper (4) is designed with an anti-bridging agitator, and a cycloidal precision feeder is arranged between the feed hopper (4) and the feeder (5), and a material seal plus nitrogen sealing is also arranged; the feeder (5) is a single-axis flexible spiral, and a 15 cm to 20 cm material seal section is arranged at the discharge end.

9. The ammonium polyvanadate coupled electrolyte preparation system according to claim 7, characterized in that: The pyrolysis reduction furnace (6) is a quantum furnace, the inner cylinder of which is made of stainless steel. The pyrolysis reduction furnace (6) is divided into a retort section, a pyrolysis section, and a reduction section. The temperature of each section is precisely controlled by the power and number of the combustion aids (7) provided in each section. The retort section of the pyrolysis reduction furnace (6) is provided with a combustion aid (7) every 1.3 m to 1.5 m, the pyrolysis section of the pyrolysis reduction furnace (6) is provided with a combustion aid (7) every 1.0 m to 1.2 m, and the reduction section of the pyrolysis reduction furnace (6) is provided with a combustion aid (7) every 0.7 m to 0.9 m.

10. The ammonium polyvanadate coupled electrolyte preparation system according to claim 7, characterized in that: The rectifier dust collector (13) is of ceramic filter element type and is provided with nitrogen periodic purge and automatic dust removal device; the gas membrane separation device (18) adopts hollow fiber membrane, and after separation, the purity of hydrogen is 92% to 98%, and the purity of nitrogen is 96% to 99.9%.

11. The ammonium polyvanadate coupled electrolyte preparation system according to claim 7, characterized in that: The combustion-supporting air heat exchanger (9) is made of stainless steel. The temperature of the high-temperature gas entering the combustion-supporting air heat exchanger (9) is 450°C to 500°C, and the temperature of the gas leaving the combustion-supporting air heat exchanger (9) is 200°C to 220°C. The temperature of the combustion-supporting air entering the combustion-supporting air heat exchanger (9) is normal temperature, and the temperature of the combustion-supporting air leaving the combustion-supporting air heat exchanger (9) is 180°C to 200°C.

12. The ammonium polyvanadate coupled electrolyte preparation system according to claim 7, characterized in that: The membrane filter (23) is a ceramic membrane or a silicon carbide membrane, and the membrane is in the form of a flat membrane or a cylindrical mold, and the accuracy of the membrane is not less than 60 μm.

Citation Information

Cited By

  • All-vanadium redox flow battery energy storage medium and preparation method and application of precursor of all-vanadium redox flow battery energy storage medium

    CN119240789A

  • Mixed acid-based electrolyte and preparation method and application thereof

    CN121355313A

  • Mixed acid-based electrolyte, preparation method and application thereof

    CN121355313B

  • Method and system for continuously producing electrolyte from ammonium metavanadate

    WO2025130814A1