Electrolyte, niobium battery including same, and method of manufacturing same

By using an electrolyte combination of polynitrile solvents and specific lithium salts in secondary batteries, combined with niobium oxide or niobium metal oxide negative electrodes, the problem of gas generation in niobium batteries is solved, achieving higher capacity retention and safety .

CN118786541APending Publication Date: 2024-10-15NYOBOLT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027083.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-04
Filing Date
2023-02-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the storage process of niobium batteries, undesirable gas formation may occur, and existing improved materials are difficult to effectively reduce gas formation.

Method used

Using an electrolyte containing a polynitrile solvent, a carbonate solvent, an ester solvent or an ether solvent, ensuring that the content of the polynitrile solvent in the electrolyte composition is at least 0.1wt%, and using a niobium oxide or niobium metal oxide negative electrode in the secondary battery, Combine specific lithium salt and solvent combinations to reduce gas production.

Benefits of technology

It effectively reduces the amount of gas generated in secondary batteries, improves the safety of niobium oxide or niobium metal oxide negative electrodes, and improves capacity retention, especially under long-term storage conditions at high temperatures and in a charged state.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786541A_ABST
    Figure CN118786541A_ABST
Patent Text Reader

Abstract

The present invention relates to a secondary battery and a method for manufacturing the same, the secondary battery comprising: a positive electrode; a negative electrode containing a niobium metal oxide; a separator between the positive electrode and the negative electrode; and an electrolyte comprising a solvent composition comprising a dinitrile solvent and at least one second solvent selected from the list consisting of mononitrile solvents, carbonate solvents, ester solvents or ether solvents wherein dinitrile is contained in an amount of at least 0.1 wt% based on the total weight of the solvent composition. The electrolyte suppresses a gas generated by a reaction between the electrolyte and the niobium metal oxide in the negative electrode, and improves the safety of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims priority to and the benefit of GB 2201480.7 filed on February 4, 2012 (04.02.2022), the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to a secondary battery and a method for preparing the secondary battery. Background Art

[0004] During storage of niobium batteries, undesirable gas generation may result. Therefore, there remains a need for improved materials for niobium-based batteries that reduce gas formation. Summary of the invention

[0005] In general, the present invention provides a secondary battery comprising an electrolyte comprising a solvent composition comprising:

[0006] a polynitrile solvent having two or more nitrile groups, and

[0007] at least one second solvent selected from the group consisting of a mononitrile solvent, a carbonate solvent, an ester solvent or an ether solvent,

[0008] The polynitrile solvent is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition.

[0009] In a first aspect of the present invention, there is provided a secondary battery comprising:

[0010] positive electrode;

[0011] a negative electrode comprising niobium oxide or niobium metal oxide;

[0012] a separator between the positive electrode and the negative electrode; and

[0013] Electrolytes, including

[0014] A solvent composition comprising:

[0015] a polynitrile solvent having two or more nitrile groups, and

[0016] at least one second solvent selected from the group consisting of mononitrile solvents, carbonate solvents, ester solvents and ether solvents,

[0017] The polynitrile solvent is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition.

[0018] In a second aspect of the present invention, there is provided a method for manufacturing a secondary battery, the method comprising:

[0019] Provide positive electrode,

[0020] providing a negative electrode comprising niobium oxide or niobium metal oxide, and

[0021] providing a separator between the positive electrode and the negative electrode; and

[0022] providing an electrolyte comprising

[0023] A solvent composition comprising:

[0024] a polynitrile solvent having two or more nitrile groups, and

[0025] at least one second solvent selected from the group consisting of a mononitrile solvent, a carbonate solvent, an ester solvent or an ether solvent,

[0026] wherein the polynitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition, and

[0027] The cathode, the anode, and the separator are brought into contact with the electrolyte to manufacture the secondary battery.

[0028] In some embodiments, the polynitrile solvent is a dinitrile solvent or a trinitrile solvent, such as a dinitrile solvent.

[0029] In some embodiments, the electrolyte further comprises a lithium salt.

[0030] In some embodiments, the negative electrode comprises niobium metal oxide.

[0031] In a specific embodiment, the polynitrile solvent is a dinitrile solvent, the electrolyte comprises a lithium salt and the negative electrode comprises a niobium metal oxide.

[0032] In some embodiments, the present invention provides a secondary battery comprising: a positive electrode; a negative electrode comprising niobium metal oxide; a separator between the positive electrode and the negative electrode; and an electrolyte, the electrolyte comprising a solvent composition and a lithium salt, the solvent composition comprising at least one of a carbonate solvent, an ester solvent or an ether solvent and a dinitrile solvent, wherein the dinitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition.

[0033] In some embodiments, the present invention provides a method for manufacturing a secondary battery, the method comprising: providing a positive electrode; providing a negative electrode comprising niobium metal oxide; and providing a separator between the positive electrode and the negative electrode; and providing an electrolyte comprising a solvent composition and a lithium salt, the solvent composition comprising at least one of a carbonate solvent, an ester solvent or an ether solvent and a dinitrile solvent, wherein the dinitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition, and contacting the positive electrode, the negative electrode and the separator with the electrolyte to manufacture the secondary battery.

[0034] The above described and other features are exemplified by the following figures and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The following drawings are of exemplary embodiments, wherein like elements are numbered the same.

[0036] Figure 1 is a graph showing the volume of gas generated in a lithium nickel cobalt aluminum oxide (NCA) / niobium tungsten oxide (NWO) pouch cell during storage of the cell for 7 days at 60°C.

[0037] Figure 2 Pie chart showing the composition of gases produced in an NCA / NOW pouch cell containing electrolyte but no salt.

[0038] Figure 3 is a graph showing the gas volume generated over time (weeks) for NCA / NOW pouch battery cells containing electrolytes with different lithium salts.

[0039] Figure 4 is a graph showing the volume of gas generated and the percentage of capacity loss in LCO / NOW pouch battery cells containing different electrolytes after the battery cells were stored at 60°C for 14 days.

[0040] Figure 5 is a graph showing the volume of gas generated and the percentage of capacity loss in LCO / NOW pouch battery cells containing different electrolytes after the battery cells were stored at 60°C for 7 days.

[0041] Figure 6 The cell volume increase of LCO / NOW pouch cells containing different electrolyte compositions after storage at 60° C. for 2 weeks (Examples 5.1 to 5.5) is shown. The black cross corresponds to the average volume increase and the shaded area corresponds to the standard deviation of the volume increase.

[0042] Figure 7 The capacity retention of LCO / NOW pouch cells containing different electrolyte compositions after storage at 60° C. for 2 weeks (Examples 5.1 to 5.5) is shown. The black cross corresponds to the average capacity retention, and the shaded area corresponds to the standard deviation of the capacity retention.

[0043] Figure 8 The cell volume increase of LCO / NOW pouch cells containing different electrolyte compositions after storage at 60° C. for 6 weeks is shown (Examples 5.2, 5.4, 5.6 and 5.7). The black cross corresponds to the average volume increase and the shaded area corresponds to the standard deviation of the volume increase.

[0044] Fig. 9 The capacity retention of LCO / NOW pouch cells containing different electrolyte compositions after storage at 60°C for 6 weeks is shown (Examples 5.2, 5.4, 5.6 and 5.7). The black cross corresponds to the average capacity retention, and the shaded area corresponds to the standard deviation of the capacity retention. DETAILED DESCRIPTION

[0045] Secondary batteries containing niobium oxide or niobium metal oxide negative electrodes produce large amounts of gas when the battery cell is in a charged state. It has been found that gas generation is affected by the composition of the electrolyte. For example, when the electrolyte contains cyclic carbonates (e.g., ethylene carbonate), reduction of the cyclic carbonates can occur in the presence of a niobium-based negative electrode. The interaction between the electrolyte and the niobium-based negative electrode can cause the electrolyte to be reduced to produce hydrogen and oxygen, especially when the battery cell is maintained in a charged state and / or at an elevated temperature. In a battery cell containing a niobium oxide or niobium metal oxide negative electrode, the decomposition of the electrolyte can be autocatalytic and involve the reaction of fluorinated salts with residual alcohols or water in the electrolyte solvent and the reduction of cyclic carbonates (if present), resulting in gas generation. The generated hydrogen and oxygen accumulate within the battery and can become hazardous.

[0046] Cells in which the negative electrode potential can be reduced to a voltage suitable for the formation of a solid-electrolyte interface (SEI) avoid this problem. For example, in cells with graphite-based negative electrodes, this gassing problem does not exist because a solid-electrolyte interface (SEI) is formed when the negative electrode potential relative to lithium is at a voltage less than 0.2 volts (V) relative to Li. The SEI is understood to passivate the negative electrode surface, avoiding electrolyte reduction. However, the SEI is also decomposed or removed at greater potentials, and therefore this strategy is not available for niobium-based electrodes because they operate at potentials greater than 0.2 V relative to Li.

[0047] Moreover, the use of sacrificial additives (e.g., vinylene carbonate or 1,3-propane sultone) in the electrolyte to promote the formation of SEI is unsatisfactory for niobium-based anodes because the battery cycles repeatedly across a range of reduction-oxidation potentials as it is charged and discharged, which causes the SEI to decompose. Furthermore, the SEI forms a resistive barrier that impedes the charge and discharge rates, thereby negatively affecting one of the key properties of niobium-based anodes.

[0048] Disclosed herein is an electrolyte that mitigates gas generation and improves the safety of a lithium ion secondary battery containing a niobium oxide or niobium metal oxide negative electrode. Specifically, it has been advantageously found that an electrolyte comprising a combination of a polynitrile solvent (e.g., a dinitrile or a trinitrile) and one or more of a carbonate, ester, and / or ether solvent effectively reduces the amount of gas generated. It is believed that the polynitrile component inhibits the decomposition of the electrolyte in the niobium metal oxide battery cell, thereby reducing the amount of gas generated.

[0049] In some embodiments, the electrolyte further comprises a lithium salt, such as a lithium salt selected from LiBF4, LiPF6, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), or a combination thereof, and additionally or alternatively lithium difluoro(oxalato)borate (LiDOFB).

[0050] In addition, it has been found that electrolytes comprising a polynitrile solvent (e.g., a dinitrile or a trinitrile) in combination with a lithium salt (e.g., LiBF4, LiPF6, or LiDFOB) and one or more carbonate, ester, and / or ether solvents further reduce the amount of gas generated. It is believed that the polynitrile solvent and the lithium salt act synergistically to further reduce electrolyte decomposition and gassing.

[0051] The present invention also results in improved capacity retention of secondary batteries due to reduced decomposition of the electrolyte, especially after prolonged storage at elevated temperatures and / or in a charged state.

[0052] Some secondary batteries and electrolytes are known, and these are discussed below.

[0053] US2017 / 0244135 describes an electrochemical battery cell and a system for restoring the capacity of the battery cell. The document discloses electrolytes comprising various solvents, such as carbonates, esters and ethers, lithium salts and additives, such as dinitriles. The embodiments disclose a battery cell comprising a graphite anode and an electrolyte of ethylene carbonate and LiTFSA (see paragraph

[0315] ). It is known that graphite anodes are not prone to gassing. US2017 / 0244135 does not disclose a niobium metal oxide negative electrode in combination with an electrolyte comprising polynitrile. The document does not discuss electrolyte gassing and does not suggest that this particular combination of polynitrile electrolyte solvent and niobium (metal) oxide anode can reduce gassing.

[0054] JP2013 / 152825 relates to reducing electrolyte decomposition and gassing. The document suggests that gassing can be reduced by using an electrolyte and / or positive electrode containing a phosphorus compound, which is capable of forming a phosphorus oxide film on the anode during the battery cell cycling process. The conventional disclosure mentions a lithium titanium niobium oxide anode and an electrolyte containing various nitrile components in combination with a phosphorus compound. The embodiments do not disclose a battery cell containing both a niobium metal oxide anode and an electrolyte containing a dinitrile, but instead focus on a Li-metal electrode with a polymer electrolyte. There is no suggestion that dinitrile is particularly effective in reducing gassing of niobium-based anodes. On the contrary, JP2013 / 152825 teaches the use of phosphorus additives to form an SEI on a Li-metal electrode. This is in contrast to the present invention, which avoids the need for an SEI, thereby enabling the battery to have better high-rate performance.

[0055] WO2020 / 047228 relates to coated cathode materials for secondary lithium-ion battery cells. The document does not provide any embodiments of complete batteries, only positive electrode materials. The conventional disclosure mentions an electrode comprising lithium niobate and an electrolyte comprising a nitrile solvent. However, there is no disclosure of an electrolyte comprising a niobium metal oxide anode and a dinitrile used in combination, and there is no mention of using the electrolyte composition to reduce gas production. The document only mentions cathode coatings or pressure repositioning systems to address gas formation.

[0056] Electrolytes

[0057] The electrolyte disclosed herein comprises a solvent composition. The solvent composition comprises a polynitrile solvent and at least one second solvent selected from the list consisting of a mononitrile solvent, a carbonate solvent, an ester solvent, or an ether solvent.

[0058] Typically, the electrolyte is non-aqueous. That is, the electrolyte contains substantially no water.

[0059] In some embodiments, the electrolyte comprises a lithium salt.

[0060] Polynitrile solvents are nitrile-containing compounds having two or more nitrile groups per molecule. Polynitrile can be C3 to C 20 Aliphatic polynitriles. Typically, the polynitriles contain 2 to 5 nitrile groups, preferably 2 to 4 nitrile groups, more preferably 2 or 3 nitrile groups. The polynitriles may be dinitriles or trinitriles.

[0061] The dinitriles are C3 to C 10 Aliphatic dinitrile, preferably C3 to C 10 Aliphatic linear dinitriles. C3 to C 10 The aliphatic group of the aliphatic dinitrile may be substituted or unsubstituted C3 to C 10 Alkyl, alkenyl or alkynyl, or preferably a straight chain C3 to C 10Alkyl, alkenyl or alkynyl. C3 to C 10 Examples of aliphatic linear dinitriles include glutaronitrile (GN; pentanedinitrile), adiponitrile (ADN; hexanedinitrile), pimelonitrile (PMN; heptanedinitrile), suberonitrile (SUN; octanedinitrile), azelanitrile (AZN; nonanedinitrile), sebaconitrile (SEN; decanedinitrile), or combinations thereof, and additionally or alternatively succinonitrile (SN; butanedinitrile),

[0062] The trinitriles are C4 to C 10 Aliphatic trinitriles, preferably C4 to C 10 Aliphatic straight chain trinitrile. C4-C 10 The aliphatic group of the aliphatic trinitrile may be substituted or unsubstituted C4-C 10 Alkyl, alkenyl or alkynyl, such as straight chain C4-C 10 Alkyl, alkenyl or alkynyl. C4-C 10 Examples of the aliphatic straight-chain trinitrile include 1,3,6-hexanetrinitrile.

[0063] Carbonate solvents include C3 to C9 linear carbonates. Examples include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), methyl isopropyl carbonate, ethyl propyl carbonate (EPC), ethyl isopropyl carbonate, ethyl methyl carbonate (EMC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), isobutylene carbonate, monofluoroethylene carbonate (FEC), 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, or combinations thereof.

[0064] In some embodiments, the solvent composition comprises a polynitrile solvent and at least one carbonate solvent. Preferably, the carbonate solvent comprises ethylene carbonate (EC), ethyl methyl carbonate (EMC), propylene carbonate (PC), or a combination thereof. More preferably, the solvent composition comprises a mixture of ethylene carbonate and ethyl methyl carbonate or propylene carbonate and ethyl methyl carbonate.

[0065] In some embodiments, the weight ratio of ethylene carbonate to ethyl methyl carbonate is from 30:70 to 50:50. In some embodiments, the weight ratio of propylene carbonate to ethyl methyl carbonate is from 30:70 to 50:50. Preferably, the weight ratio is about 30:70.

[0066] Preferably, the solvent composition comprises a propylene carbonate (PC) solvent. In some such embodiments, the propylene carbonate is included in an amount of at least 1 wt % based on the total weight of the solvent composition.

[0067] The ether solvent includes dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0068] The ester solvent includes C3 to C9 straight chain esters. Examples include methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, 5-decanolide, γ-valerolactone, dl-mevalonolactone, γ-caprolactone, or a combination thereof.

[0069] The polynitrile solvent (e.g., dinitrile or trinitrile solvent) is included in the solvent composition in an amount of at least 0.1 wt %, such as at least 0.5 wt %, or at least 1 wt %, or at least 5 wt %, or at least 10 wt %. In one aspect, based on the gross weight of the solvent composition, the dinitrile solvent is included in the solvent composition in an amount of 0.1 wt % to 55 wt %, or 0.2 wt % to 50 wt %, or 1 wt % to 45 wt %, or 5 wt % to 40 wt %, or 5 wt % to 30 wt %, or 10 wt % to 30 wt %, or 10 wt % to 25 wt %, or 10 wt % to 20 wt %.

[0070] Preferably, the dinitrile solvent is included in the solvent composition in an amount of at least 0.1 wt %, such as at least 0.5 wt %, or at least 1 wt %, or at least 5 wt %, or at least 10 wt %. In an embodiment, based on the total weight of the solvent composition, the dinitrile solvent is included in the solvent composition in an amount of 0.1 wt % to 55 wt %, or 0.2 wt % to 50 wt %, or 1 wt % to 45 wt %, or 5 wt % to 40 wt %, or 5 wt % to 30 wt %, or 10 wt % to 30 wt %, or 10 wt % to 25 wt %, or 10 wt % to 20 wt %.

[0071] In one embodiment, the polynitrile solvent is included in the solvent composition in an amount of about 10 wt % to about 50 wt %, preferably about 20 wt % to about 40 wt %, based on the total weight of the solvent composition.

[0072] In another embodiment, the polynitrile solvent is included in the solvent composition in an amount of 1 wt % to 10 wt %, preferably 2 wt % to 5 wt %, more preferably about 5 wt %, based on the total weight of the solvent composition.

[0073] In one aspect, the total amount of mononitrile solvents, carbonate solvents, ester solvents, and / or ether solvents contained in the solvent composition is from 1 wt % to 99.8 wt %, or from 20 wt % to 99.8 wt %, or from 30 wt % to 99 wt %, or from 40 wt % to 95 wt %, or from 50 wt % to 95 wt %, or from 70 wt % to 90 wt %, or from 75 wt % to 90 wt %, or from 80 wt % to 90 wt %, based on the total weight of the solvent composition.

[0074] In one aspect, the weight ratio of the dinitrile solvent to the total amount of the mononitrile solvent, carbonate solvent, ester solvent and / or ether solvent can be 5:1 to 1:20, or 3:1 to 1:20, or 2:1 to 1:10, or 1:1 to 1:10, or 1:2 to 1:10, or 1:3 to 1:10.

[0075] In one aspect, the solvent composition comprises a carbonate solvent. In one aspect, the carbonate solvent comprises PC, EMC or a combination thereof. In one aspect, the carbonate solvent consists of PC, EMC or a combination thereof. In one aspect, the carbonate comprises EC or PC, and based on the gross weight of the solvent composition, comprises EC or PC in an amount of at least 1wt%. In one aspect, based on the gross weight of the solvent composition, comprises EC or PC in an amount of at least 1wt%, at least 5wt%, at least 10wt%, or at least 20wt%. In one aspect, based on the gross weight of the solvent composition, comprises EC or PC in an amount of 1wt% to 60wt%, or 5wt% to 45wt%, or 10wt% to 40wt%.

[0076] In one aspect, the solvent composition includes a mononitrile solvent. In one aspect, the mononitrile solvent includes a C2 to C8 aliphatic mononitrile. The aliphatic group of the C2 to C8 aliphatic mononitrile can be a straight or branched C2 to C8 alkyl, alkenyl or alkynyl, and in one aspect, a straight C2 to C8 alkyl, alkenyl or alkynyl. The embodiment of the mononitrile includes methoxypropionitrile, butyronitrile, acetonitrile, propanenitrile (propanenitrile) (proprionitrile), acetonitrile or a combination thereof. In one aspect, based on the gross weight of the solvent composition, the mononitrile solvent is included in the solvent composition in an amount of 1 wt% to 95 wt%, or 5 wt% to 90 wt%, or 10 wt% to 85 wt%, or 10 wt% to 75 wt%, or 20 wt% to 50 wt%. In one aspect, the mononitrile solvent is included in the solvent composition in an amount of 5wt% to 50 wt%, or 10 wt% to 40 wt%.

[0077] In one aspect, the solvent composition comprises a dinitrile solvent and a mononitrile solvent, and based on the gross weight of the solvent composition, the total amount of carbonate solvents, ether solvents, and ester solvents in the solvent composition is 0.01 wt % to 10 wt %, or 0.05 wt % to 5 wt %, or 0.1 wt % to 1 wt %. In one aspect, the solvent composition comprises a dinitrile solvent and a mononitrile solvent, and is substantially free of carbonate solvents, ester solvents, or ether solvents.

[0078] In one aspect, the solvent consists of PC or EC, EMC, and ADN. In one aspect, the solvent composition comprises or consists of 30 wt % PC or EC, 60 wt % EMC, and 10 wt % ADN.

[0079] In a preferred embodiment, the solvent composition comprises, for example, consists of PC or EC, EMC, and ADN, SN or TN. In such an embodiment, the solvent composition comprises, or consists of, PC or EC, and EMC in a weight ratio of 30:70 to 50:50, and ADN, SN or TN in an amount of 2 wt.% to 5 wt.% based on the weight of the electrolyte composition.

[0080] In a particularly preferred embodiment, the solvent composition comprises, for example, consists of PC, EMC, and ADN, SN or TN. In such an embodiment, the solvent composition comprises, or consists of, PC and EMC in a weight ratio of 30:70 to 50:50, and ADN, SN or TN in an amount of 2 wt.% to 5 wt.% based on the weight of the electrolyte composition.

[0081] In another preferred embodiment, the solvent composition comprises, for example, consists of PC, EMC, and ADN or SN. In such an embodiment, the solvent composition comprises, or consists of, PC and EMC in a weight ratio of 30:70 to 50:50, and ADN or SN in an amount of 2 wt.% to 5 wt.% based on the weight of the electrolyte composition. In a more preferred embodiment, the dinitrile is SN.

[0082] In some embodiments, the electrolyte comprises a lithium salt.

[0083] In some such embodiments, the lithium salt in the electrolyte includes LiBF4, LiPF6, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), or a combination thereof, and additionally or alternatively lithium difluoro(oxalate)borate (LiDOFB). The concentration of the lithium salt in the (e.g., non-aqueous) electrolyte is based on the total weight of the electrolyte, for example, 0.01 molar (M) to 2.0 M, 0.05 M to 1.8 M, 0.1 M to 1.6 M, 0.5 M to 1.4 M, 0.5 M to 1.3 M, or 0.8 M to 1 M. In one embodiment, the lithium salt includes 0.01 to 1 M LiBF4 and 0.1 M to 0.3 M LiPF6. In another embodiment, the lithium salt includes 0.1 to 0.3 M LiBF4, such as 0.2 M LiBF4. In another embodiment, the lithium salt comprises 0.05 to 0.2 M LiDFOB, such as 0.1 M LiDFOB.

[0084] In one aspect, the electrolyte comprises 0.5 M to 3 M of a lithium salt and is substantially free of PF6 - In one aspect, the electrolyte comprises less than 0.1 M, or less than 0.05 M, or less than 0.02 M, or less than 0.01 M, or less than 0.005 M PF6 - In one aspect, the electrolyte does not contain PF6 - .

[0085] The solvent composition may be prepared by combining at least one of a carbonate solvent, an ester solvent, or an ether solvent and a dinitrile solvent. The electrolyte may be prepared by contacting the solvent composition with a lithium salt (when present) and dissolving the lithium salt in the solvent composition.

[0086] Secondary battery

[0087] A secondary battery comprising the electrolyte described herein is also disclosed. In particular, the secondary battery comprises: a positive electrode; a negative electrode comprising niobium metal oxide; a separator between the positive electrode and the negative electrode; and an electrolyte. Typically, a battery comprises one or more electrochemical cells. In general, a secondary battery refers to a battery in which the cell reaction is reversible, so the battery is typically rechargeable.

[0088] The negative electrode includes a negative electrode active material on a current collector. The negative electrode active material includes niobium oxide or niobium metal oxide. Typically, the negative electrode active material is mainly composed of niobium oxide or niobium metal oxide.

[0089] Niobium metal oxides generally have the formula Nb x M y O z , wherein x is 2 to 34, y is 1 to 20, and z is 8 to 115, and M is Na, Mg, Al, Si, P, S, K, Ca, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, As, Y, Zr, Mo, In, Sn, Sb, Ta, W, or a combination thereof. In one aspect, M is V, Cr, Mo, Ta, W, P, S, or a combination thereof. In one aspect, the niobium metal oxide comprises niobium, tungsten, or molybdenum, and optionally calcium, chromium, cobalt, magnesium, manganese, nickel, potassium, phosphorus, sodium, sulfur, or a combination thereof. In one aspect, the niobium metal oxide is niobium tungsten oxide or niobium molybdenum oxide. In one aspect, the niobium metal oxide comprises niobium, tungsten, or molybdenum and oxygen. Examples of niobium tungsten oxides include Nb 14 W3O 44 , Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 、Nb2Mo3O 14 , Nb 14 Mo3O 44 , Nb 12 MoO 44 or a combination thereof. In one aspect, the niobium metal oxide comprises Nb 16 W5W 55 .

[0090] Niobium oxides generally have the formula Nb x1 O z1 , wherein x1 is 2 to 25 and z1 is 2 to 62. Examples of niobium oxides include Nb2O5, NbO2, Nb 12 O 29or Nb2O 62 or a combination thereof.

[0091] It is also mentioned that niobium oxide is doped to provide a material of the formula Nb x M1 y1 M2 y2 O z Aspects of the compounds wherein M1 is W or Mo, M2 is V, Cr, Mo, Ta, W, P, S or a combination thereof, x is 2 to 34, (y1+y2) is 1 to 20, and z is 8 to 115, 0≤y1≤20 and 0≤y2≤20.

[0092] The negative electrode active material may further include an additional active material. Examples of additional negative electrode active materials include tungsten oxide, lithium titanium oxide, or a combination thereof.

[0093] The negative electrode can be formed by a negative electrode composition comprising a negative electrode active material. In addition to the negative electrode active material, the negative electrode composition can further include a binder, a solvent, a conductive agent, or a combination thereof. The binder can include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, or a combination thereof. The conductive agent can include conductive carbon such as carbon nanotubes, natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber, or metals such as copper, nickel, aluminum, or silver powder or fiber.

[0094] In one aspect, the negative electrode comprises a negative electrode composition disposed on an aluminum current collector, the negative electrode composition comprising Nb as a negative electrode active material. 16 W5W 55 , SBR as a binder, and conductive carbon as a conductive agent, or consisting of the above.

[0095] Alternatively, the negative electrode current collector may include copper, nickel, stainless steel, carbon steel, titanium, or combinations thereof.

[0096] The negative electrode may be formed by coating a layer of the negative electrode composition on a negative electrode collector, or alternatively, the negative electrode composition may be cast on a separate support and a film layer peeled off from the separate support may be laminated on a metal current collector. The method for preparing the negative electrode is not limited thereto, and any other method suitable for preparing the negative electrode may also be used.

[0097] The positive electrode includes a positive electrode active material. The positive electrode may include lithium cobalt oxide (LCO), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide (LMO), lithium nickel manganese oxide (LNMO), lithium nickel cobalt manganese oxide (NMC) (e.g., LiNi 0.8 Co 0.10 Mn 0.10 O2; NMC811), lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP) or a combination thereof. Preferably, the positive electrode active material comprises LCO, NCA or NMC.

[0098] The positive electrode can be formed from a positive electrode composition containing a positive electrode active material. In addition to the positive electrode active material, the positive electrode composition may further include a binder, a solvent, a conductive agent, or a combination thereof. The conductive agent may include carbon nanotubes, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, metals such as copper, nickel, aluminum, or silver powder or fibers, or a combination thereof. The binder in the positive electrode composition may include polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, or a combination thereof. In one aspect, the positive electrode includes a positive electrode composition on an aluminum current collector, the positive electrode composition comprising NMC or LCO as a positive electrode active material, PVDF as a binder, and carbon nanotubes, carbon black, and / or ketjen black as a conductive agent, or a combination thereof.

[0099] The positive electrode may further include a positive electrode current collector including aluminum, titanium, stainless steel, carbon, or a combination thereof.

[0100] The positive electrode can be prepared in a manner similar to that described above for the negative electrode.

[0101] The secondary battery includes a separator between the positive electrode and the negative electrode. The separator is not limited and can be any separator suitable for lithium-ion batteries. The separator includes a separator material that is electrically insulating, non-chemically reactive with the positive electrode active material and the negative electrode active material, non-chemically reactive with the electrolyte, and insoluble in the electrolyte. In addition, the separator material is selected so that it has a porosity sufficient to allow the electrolyte to flow through during the electrochemical reaction of the battery cell. The separator can be a porous polymer film, or can be a non-woven or woven fabric. The separator can include, for example, polypropylene (e.g., Celgard® 2500), polyethylene, polyamide (nylon), polysulfone, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-hydrogen fluoride propylene (PVDF-HFP), tetrafluoroethylene-ethylene copolymer (PETFE), chlorotrifluoroethylene-ethylene copolymer, or a combination thereof. In one aspect, the separator can include two or more layers of alternating materials, for example, a three-layer separator of polypropylene / polyethylene / polypropylene. The separator can be impregnated with an electrolyte.

[0102] Preparation method

[0103] The battery cell is manufactured by providing a nonaqueous electrolyte and adding the nonaqueous electrolyte to an assembly including a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode.

[0104] The secondary battery may have any configuration, such as a cylindrical wound cell, a prismatic cell, a rigid laminar cell, or a flexible soft pack cell, a jacket cell, or a pouch cell.

[0105] The secondary battery disclosed herein comprising niobium metal oxide as a negative electrode active material and an electrolyte exhibits reduced gas generation. Specifically, during extended storage at a temperature of 50°C to 70°C, or 55°C to 65°C, or 60°C, the secondary battery produces a relatively small amount of gas. Based on the total volume of the battery cell, after storing the secondary battery at 60°C for 6 days, the disclosed secondary battery has a gas generation volume of less than 10 vol%, or less than 8 vol%, or less than 5 vol%, or less than 3 vol%, or less than 1 vol%, or less than 0.1 vol%. Based on the total volume of the battery cell, after being stored at 60°C for 14 days, the disclosed secondary battery also has a gas generation volume of 0.001 vol%, 0.01 vol%, or 0.1 vol% to 1 vol%, 5 vol%, or 10 vol%. In one aspect, the gas volume is less than 10% of the total battery cell volume after being stored at 60°C for 3 months.

[0106] The present disclosure is further illustrated by the following examples, which are non-limiting.

[0107] Other options

[0108] Each and every compatible combination of the above-described embodiments are expressly disclosed herein as if each and every combination were individually and expressly set forth.

[0109] Various further aspects and embodiments of the present invention will be apparent to those skilled in the art in view of this disclosure.

[0110] As used herein, "and / or" should be considered as specific disclosure of each of two specific features or components with or without the other. For example, "A and / or B" should be considered as specific disclosure of each of (i) A, (ii) B, and (iii) A and B, just as if each were individually set forth herein.

[0111] Unless the context dictates otherwise, the descriptions and definitions of the features set out above are not limited to any particular aspect or embodiment of the invention, and apply equally to all aspects and embodiments described.

[0112] Certain aspects and embodiments of the invention will now be described by way of example and with reference to the above-mentioned drawings.

[0113] Alternatively, the compositions, methods and articles may comprise, consist of or consist essentially of any suitable material, step or component disclosed herein. The compositions, methods and articles may additionally or alternatively be formulated so as to be free of or essentially free of any material (or substance), step, or component that is not necessary to achieve the function or purpose of the compositions, methods and articles.

[0114] It will be understood that when an element is referred to as being “on” another element, it can be directly on the other element or intervening elements may be present therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements present.

[0115] All ranges disclosed herein include endpoints, and the endpoints can be combined independently of each other (e.g., "up to 25 wt.%, or more specifically, 5 wt.% to 20 wt.%" includes endpoints and all intermediate values ​​of the "5 wt.% to 25 wt.%" range, etc.). "Combination" includes blends, mixtures, alloys, reaction products, etc. The terms "first", "second", etc. do not indicate any order, quantity, or importance, but are used to distinguish one element from another. Unless otherwise indicated herein or clearly contradicted by the context, the terms "one", "an", and "the" do not indicate a limit on quantity, but are interpreted to cover both the singular and the plural. Unless otherwise expressly stated, "or" means "and / or". References throughout the specification to "some embodiments", "embodiments", etc. refer to specific elements described in conjunction with the embodiments, which are included in at least one embodiment described herein, and may or may not be present in other embodiments. In addition, it should be understood that the described elements can be combined in various embodiments in any suitable manner. "Combinations thereof" is open ended and includes any combination comprising at least one of the listed components or properties, optionally together with unlisted similar or equivalent components or properties.

[0116] Unless otherwise limited, the technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the application belongs. All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term in the present application contradicts or conflicts with a term in the combined reference, the term from the present application takes precedence over the conflicting term from the combined reference.

[0117] Compounds are described using standard nomenclature. For example, any position not substituted by any indicated group is understood to have its valency filled by the indicated bond or hydrogen atom. A dash ("-") that is not between two letters or symbols is used to indicate the point of attachment of a substituent. For example, -CHO is attached through the carbon of the carbonyl group.

[0118] "Aliphatic" or "aliphatic group" refers to a saturated or unsaturated straight or branched chain hydrocarbon group. An aliphatic group can be an alkyl, alkenyl, or alkynyl group. For example, "nitrile" or "mononitrile" refers to a compound having the formula R-CN, wherein R is a substituted or unsubstituted C2-C 20 Aliphatic groups. "Dinitrile" refers to compounds having the formula CN-R-CN, where R is a substituted or unsubstituted C2-C 20 Aliphatic group.

[0119] "Cyclic carbonate" refers to a carbonate compound having at least one ring and wherein the carbonate group (-O(C=O)O-) forms part of the ring. "Acyclic carbonate" refers to a carbonate compound wherein the carbonate group (-O(C=O)O-) does not form part of the ring. Acyclic carbonates may include straight hydrocarbon chains, branched hydrocarbon chains, or both.

[0120] The term "alkyl" refers to a branched or straight chain, unsaturated aliphatic hydrocarbon group, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, sec-pentyl, and n-hexyl and sec-hexyl.

[0121] "Alkenyl" refers to a straight or branched monovalent hydrocarbon radical having at least one carbon-carbon double bond (eg, ethenyl (-HC=CH2)).

[0122] "Alkylene" refers to a straight or branched, saturated, divalent aliphatic hydrocarbon group (eg, methylene (-CH2-) or propylene (-(CH2)3-)).

[0123] "Substituted" refers to a substituted compound or group in which hydrogen is replaced with at least one (e.g., 1, 2, 3, 4, 5, 6 or more) substituent independently selected from the group consisting of halogen (e.g., F-, Cl-, Br-, I-), hydroxy, alkoxy, nitro, cyano, amino, azido, amidino, hydrazine, hydrazone, carbonyl, carbamoyl, thiol, C1 to C6 alkoxycarbonyl, ester, carboxyl, or a salt thereof, sulfonic acid or a salt thereof, phosphoric acid or a salt thereof, C1 to C6 alkoxycarbonyl, ester, carboxyl, or a salt thereof, sulfonic acid or a salt thereof, phosphoric acid or a salt thereof, or a C1 to C6 alkoxycarbonyl group. 20 Alkyl, C2 to C 16 Alkynyl, C6 to C 20 Aryl, C7 to C 13 Aralkyl, C1 to C4 oxyalkyl, C1 to C 20 Heteroalkyl, C3 to C 20 Heteroaryl (i.e., a group containing at least one aromatic ring in which at least one ring member is not carbon), C3 to C 20 Heteroarylalkyl, C3 to C 20 Cycloalkyl, C3 to C 15 Cycloalkenyl, C6 to C 15 Cycloalkynyl, C5 to C 15 Heterocycloalkyl, or a combination comprising at least one of the foregoing, so long as the normal valency of the substituted atom is not exceeded.

[0124] Although specific embodiments have been described, the applicant or other persons skilled in the art may think of alternatives, modifications, variations, improvements, and substantial equivalents that are not currently foreseeable or may not be foreseeable. Therefore, the appended claims submitted and that may be amended are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.

[0125] Description of the Invention

[0126] The following numbered paragraphs contain statements of broad combinations of technical features according to various aspects of the invention disclosed herein.

[0127] 1. A secondary battery comprising:

[0128] positive electrode;

[0129] a negative electrode comprising niobium metal oxide;

[0130] a separator, located between the positive electrode and the negative electrode; and

[0131] Electrolytes, including

[0132] A solvent composition comprising at least one of a mononitrile solvent, a carbonate solvent, an ester solvent or an ether solvent and a dinitrile solvent, wherein the dinitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition, and

[0133] Lithium salts.

[0134] 2. The secondary battery according to paragraph 1, wherein the dinitrile is C3 to C 10 Aliphatic linear dinitriles.

[0135] 3. The secondary battery according to paragraph 2, wherein the C3 to C 10 The aliphatic straight-chain dinitriles include glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile, sebacononitrile or a combination thereof.

[0136] 4. The secondary battery according to paragraph 2, wherein the C3 to C 10 The aliphatic straight-chain dinitrile is adiponitrile.

[0137] 5. The secondary battery according to any one of paragraphs 1 to 4, wherein the dinitrile is contained in an amount of 0.2 wt % to 50 wt % based on the total weight of the solvent composition.

[0138] 6. A secondary battery according to any one of paragraphs 1 to 5, wherein the carbonate solvent comprises dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, ethylmethyl carbonate, ethylmethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, or a combination thereof.

[0139] 7. The secondary battery according to paragraph 6, wherein the carbonate solvent includes propylene carbonate, and the propylene carbonate is included in an amount of at least 1 wt % based on the total weight of the solvent composition.

[0140] 8. The secondary battery according to any one of paragraphs 1 to 7, wherein the ester solvent comprises methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, 5-decanoic acid lactone, γ-valerolactone, dl-mevalonolactone, γ-caprolactone, or a combination thereof.

[0141] 9. The secondary battery according to any one of paragraphs 1 to 8, wherein the ether solvent comprises dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0142] 10. The secondary battery according to any one of paragraphs 1 to 9, wherein the mononitrile solvent comprises a C2 to C8 aliphatic mononitrile.

[0143] 11. The secondary battery according to paragraph 9, wherein the C2 to C8 aliphatic mononitrile comprises butyronitrile, acetonitrile, propionitrile, acetonitrile, or a combination thereof.

[0144] 12. The secondary battery according to paragraph 10, wherein the C2 to C8 aliphatic mononitrile is included in an amount of 30 to 90 wt % based on the total weight of the solvent composition.

[0145] 13. The secondary battery according to any one of paragraphs 1 to 12, wherein the lithium salt comprises LiBF4.

[0146] 14. The secondary battery according to any one of paragraphs 1 to 13, wherein the lithium salt is contained in the electrolyte at a concentration of 0.5 to 3 mol / L.

[0147] 15. The secondary battery according to paragraph 14, wherein the electrolyte comprises 0.01 to 0.3 mol / L of LiBF4.

[0148] 16. The secondary battery according to paragraph 14, wherein the electrolyte comprises 0.8 mol / L to 3 mol / L of LiPF6.

[0149] 17. A secondary battery according to paragraph 14, wherein the electrolyte contains less than 0.1 mol / L of PF6 - .

[0150] 18. The secondary battery according to paragraph 14, wherein the electrolyte does not contain PF6 - .

[0151] 19. A secondary battery according to any one of paragraphs 1 to 18, wherein the niobium metal oxide is Nb 14 W3O 44 , Nb 16 W5W 55 , Nb18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 、Nb2Mo3O 14 , Nb 14 Mo3O 44 , Nb 12 MoO 44 or a combination thereof.

[0152] 20. The secondary battery according to paragraph 19, wherein the niobium metal oxide is Nb 16 W5W 55 .

[0153] 21. A method for manufacturing a secondary battery, the method comprising:

[0154] Provide positive electrode,

[0155] providing a negative electrode comprising a niobium metal oxide, and

[0156] providing a separator between the positive electrode and the negative electrode; and

[0157] Providing an electrolyte comprising

[0158] A solvent composition comprising at least one of a carbonate solvent, an ester solvent, or an ether solvent and a dinitrile solvent, wherein the dinitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition, and

[0159] Lithium salts, and

[0160] The cathode, the anode, and the separator are brought into contact with the electrolyte to manufacture the secondary battery.

[0161] Example

[0162] The following examples are provided to further illustrate the present invention and are not intended to limit the scope of the present invention.

[0163] Example 1

[0164] The positive electrode active material is lithium nickel cobalt aluminum oxide (LiNi x Co y Al z O2, where x ≥ 0.8, z ≤ 0.05 and x + y + z = 1, NCA) and niobium tungsten oxide Nb as the negative electrode active material 16 W5W 55A multilayer pouch cell of (NWO) was filled with an electrolyte containing 1 M LiPF6 and solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a 30:70 EC:EMC weight ratio and charged to 3 V. The electrode stack was extracted from the charged full cell and separated into individual anode layers, each with a capacity of about 80 mAh. In this state, the NWO anode was fully lithiated and at a potential of ~1.1 V vs. lithium.

[0165] The first negative electrode layer (1) was not rinsed and placed in a pouch with fresh electrolyte, the second negative electrode layer (2) was rinsed and placed in a pouch with fresh electrolyte, and the third negative electrode layer (3) was rinsed and placed in a pouch with only 30:70 EC:EMC solvent (i.e., no LiPF6 salt).

[0166] Figure 1 The volume of gas produced by the interaction between the NWO anode and the other materials contained in the pouch (i.e., electrolyte in the case of layers (1) and (2) and solvent in the case of layer (3)) is shown. Layer (1), which was not flushed and therefore had a higher salt concentration, produced the highest volume of gas. Layer (2), which was flushed and then in contact with a 30:70 EC:EMC electrolyte, produced a lower volume of gas, but the volume was still greater than that produced by layer (3). Thus, reduced salt concentrations (1>2>3) lead to reduced gas volumes as the autocatalytic decomposition of LiPF6 is less significant.

[0167] Example 2

[0168] The composition of the gas generated by the salt-free pouch (third negative electrode layer) in Example 1 was measured by gas chromatography to determine the role of the solvent in gas generation independent of the salt. The results are shown in Figure 2 In the graph, it can be seen that a significant percentage of the gas is composed of ethylene (the gas is composed of 90% hydrogen, 3% carbon dioxide, 7% ethylene), which indicates a reduction in the EC of the electrolyte solvent. It was concluded from these experiments that benefits can be obtained by using salt and solvent packaging that are tailored to reduce interactions with the NWO anode.

[0169] Example 3

[0170] The effect of lithium salts on gas generation was evaluated. Multilayer 0.6 ampere-hour (Ah) NCA / NOW soft pack cells were prepared and filled with one of the following electrolytes: 1 M LiPF6 and 30:70 EC:EMC, 1 M LiFSI and 30:70 EC:EMC, or 1 M LiBF4 and 30:70 EC:EMC. The cells were charged to 3 V, leaving the NWO anode fully lithiated and at a potential of approximately 1.1 V relative to lithium. The cells were stored in a 60°C oven and the gas volume was measured periodically as described in Example 1.

[0171] result( Figure 3 ) showed that the use of LiBF4 salt significantly reduced gas generation compared to LiPF6 or LiFSI.

[0172] Example 4

[0173] The effect of electrolyte solvents on gas generation was evaluated. Multilayer 0.16 Ah LCO / NOW soft pack battery cells were filled with electrolytes containing 1.1 M of 20% LiBF4 / 80% LiPF6 salt in different solvents, formed, and charged to 3.35 V or 3.25 V. A mixture of LiBF4 / LiPF6 was used instead of pure LiBF4 to provide improved electrolyte conductivity while avoiding gas generation. Based on the stability of the solvents adiponitrile (ADN), propionitrile (PN), and propylene carbonate (PC) relative to lithium at low voltage for reduction, these solvents were tested. The electrolyte compositions tested are shown in Table 1 below. Once assembled, the pouches were stored at 60 ° C for 14 days and the gas volume was measured as described in Example 1. The capacity of the battery cell was also measured by discharging to 1.3 V at C / 2 and compared with the initial capacity.

[0174] Table 1

[0175]

[0176] like Figure 4 As shown, when the solvent was 20:40:40 PC:EMC:ADN, the battery cells charged to 3.35 V showed significantly less gas generation and lower capacity loss, indicating the stability of this solvent system. When charged to 3.25 V, the battery cells containing the 45:45:10 blend of PC:EMC:ADN had less gas generation and lower capacity loss than the battery cells containing the 30:70 blend of EC:EMC. These battery cells also had less gas generation and capacity loss than the 50:50 blend of PC:EMC, indicating that ADN significantly improved the solvent stability.

[0177] Replacing 10% of the EMC in 45:45:10 PC:EMC:ADN with PN in order to reduce viscosity. Storing the cells at 60°C for 7 days resulted in minimal gas generation and capacity loss. Figure 5 The results in show that PN improves the electrochemical performance of battery cells containing PC and ADN.

[0178] As demonstrated in the examples, use of selected salt and solvent combinations provides reduced gas generation for niobium oxide or niobium metal oxide negative electrodes.

[0179] Example 5

[0180] Additional tests were conducted to test electrolyte compositions with alternative electrode materials and alternative nitrile solvents.

[0181] In Examples 5.1 to 5.7, lithium cobalt oxide (LiCoO2, LCO) was used as the positive electrode active material (cathode during discharge), niobium tungsten oxide (Nb2O3, LCO) was used as the negative electrode active material (anode during discharge), and niobium tungsten oxide (Nb2O3, LCO) was used as the negative electrode active material (anode during discharge). 16 W5W 55 , NWO), a polyethylene separator and an electrolyte to prepare a multilayer 0.12 ampere-hour (Ah) soft pack battery cell. The electrodes were each arranged on an aluminum current collector and assembled in a soft pack battery cell together with a separator. The soft pack battery cell was filled with an electrolyte composition and vacuum sealed.

[0182] The electrolyte comprises a base solvent which is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and / or propylene carbonate (PC) in the weight ratios listed in Table 2. Example 5.1 was prepared without any other electrolyte additives. Example 5.2 comprises a lithium salt (LiBF4) as an additive present in the electrolyte at a molar concentration of 0.2 M (see Table 2). Examples 5.3 to 5.7 comprise a dinitrile solvent selected from adiponectin (ADN) and succinonitrile (SN) or a trinitrile solvent (TN) which is 1,3,6-hexanetrinitrile. The amount of the nitrile solvent included is indicated in Table 2 as a weight percentage of the total electrolyte solution.

[0183] Table 2

[0184]

[0185] The pouch cell had initial outer dimensions of 50 mm × 34 mm × 3 mm. The initial volume of the cell was determined by measuring the total displacement of the cell in the fluid (Archimedes principle). The cell was then charged to 3.15 V at room temperature and discharged to 1.3 V at a C rate of C / 2 to determine the initial discharge capacity.

[0186] The cells were recharged to 3.15 V and stored in a 60°C oven for 6 weeks.

[0187] The gas volume in the battery cell was measured after 2 weeks of storage and after 6 weeks of storage. To measure the gas volume, the battery power source was removed from the oven and allowed to cool to room temperature. The volume of the battery cell was then measured as described above. The battery cell volume increase (%) was calculated by comparing the battery cell volume at 2 weeks or 6 weeks with the initial volume.

[0188] Figure 6 The cell volume increase of Examples 5.1 to 5.5 after 2 weeks of storage at 60° C. is shown. The black cross corresponds to the mean volume increase and the shaded area corresponds to the standard deviation.

[0189] Figure 8 The cell volume increase is shown for Examples 5.2, 5.4, 5.6 and 5.7 after 6 weeks of storage at 60° C. The black cross corresponds to the mean volume increase and the shaded area corresponds to the standard deviation.

[0190] After 2 weeks, Example 5.1 (no additive) had a volume increase of over 14%. In contrast, Examples 5.3, 5.4, and 5.5 (2% ADN, SN, and TN) only showed a volume increase of 8% to 12% in 2 weeks. Dinitrile and trinitrile additives are believed to suppress gas generation, thus preventing large cell volume increases. It is shown that dinitrile ADN and SN suppress cell volume increases better than trinitrile additives.

[0191] After 6 weeks, Example 5.4 (2% SN) showed a volume increase of 35%, but Examples 5.6 and 5.7 (both 5% SN) had lower volume increases of about 23% and 4%, respectively. Inclusion of higher amounts of dinitrile (SN) showed further suppression of gas generation and thus resulted in a small cell volume increase. Specifically, the combination of PC / EMC base solvent with 5% SN additive (Example 5.7) showed a significant reduction in cell volume increase to only 4% within 6 weeks.

[0192] Example 5.2 (0.2M LiBF4) shows a low volume increase of about 4% in 2 weeks and about 10% in 6 weeks. However, the volume increase observed for Example 5.7 (PC / EMC and 5% SN) is lower in 6 weeks, and the capacity retention of Example 5.2 is worse than all the dinitrile / trinitrile containing electrolytes, as discussed below.

[0193] The discharge capacity of the battery cells was measured after 2 weeks of storage and after 6 weeks of storage. To measure the discharge capacity, the battery cells were removed from the oven and allowed to cool to room temperature. The battery cells were discharged to 1.3 V at a C rate of C / 2 to determine the discharge capacity. The discharge capacity retention (%) was calculated by comparing the 2-week or 6-week discharge capacity with the initial discharge capacity.

[0194] Figure 7 The capacity retention of Examples 5.1 to 5.5 after 2 weeks of storage at 60° C. is shown. The black cross corresponds to the average capacity retention, and the shaded area corresponds to the standard deviation.

[0195] Fig. 9 The capacity retention of Examples 5.2, 5.4, 5.6 and 5.7 after 6 weeks of storage at 60° C. The black cross corresponds to the average capacity retention and the shaded area corresponds to the standard deviation.

[0196] After 2 weeks, Example 5.1 (no additive) had a capacity retention of about 16%. Examples 5.3, 5.4, and 5.5 (2% ADN, SN, and TN) showed better capacity retention of 64%, 71%, and 54%, respectively. In particular, the capacity retention of Example 5.4 (2% SN) was higher than all other examples within 2 weeks. This is believed to be due to the suppression of electrolyte gas generation by the dinitrile and trinitrile additives.

[0197] Over 6 weeks, Example 5.4 (2% SN) showed a capacity retention of 39%, while Examples 5.6 and 5.7 (both 5% SN) had higher capacity retentions of 62% and 64%, respectively. Inclusion of higher amounts of dinitrile (SN) was shown to further suppress gas generation, resulting in improved capacity retention.

[0198] Example 5.2 (0.2M LiBF4) showed reasonable capacity retention (69%) over 2 weeks, however, this dropped to only 25% after 6 weeks. Examples containing nitrile additives, such as Examples 5.4, 5.6 and 5.7 all had better capacity retention over the longer 6 week period (39%, 62% and 64%, respectively).

[0199] These examples show that adding a dinitrile or trinitrile solvent to the electrolyte provides a good balance of performance (both lower cell volume increase and higher capacity retention) over long term storage of the cell. However, the examples (e.g., Example 4) also show that adding both a lithium salt and a dinitrile or trinitrile solvent provides even further improvements to electrolyte gas generation and capacity retention.

[0200] References

[0201] Many publications are cited above to more fully describe and disclose the present invention and the current state of the art to which the present invention belongs. The complete citations of these references are provided below. The entire contents of each of these references are incorporated herein.

[0202] US 2017 / 0244135

[0203] JP 2013 / 152825

[0204] WO 2020 / 047228.

Claims

1. A secondary battery comprising: positive electrode; a negative electrode comprising niobium oxide or niobium metal oxide; a separator between the positive electrode and the negative electrode; and Electrolytes, including A solvent composition comprising: a polynitrile solvent having two or more nitrile groups, and at least one second solvent selected from the group consisting of mononitrile solvents, carbonate solvents, ester solvents and ether solvents, The polynitrile solvent is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition. 2 . The secondary battery according to claim 1 , wherein the polynitrile solvent is a dinitrile solvent or a trinitrile solvent, preferably a dinitrile solvent.

3. The secondary battery according to claim 1 or 2, wherein the polynitrile solvent is C3 to C 10 Aliphatic dinitrile, preferably C3 to C 10 Aliphatic straight chain dinitrile.

4. The secondary battery according to claim 3, wherein the C3 to C 10 The aliphatic dinitriles include glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile, sebacononitrile, succinonitrile or a combination thereof.

5. The secondary battery according to claim 3, wherein the C3 to C 10 The aliphatic dinitrile is adiponitrile or succinonitrile.

6. The secondary battery according to claim 1 or claim 2, wherein the polynitrile solvent is C4 to C 10 Aliphatic trinitriles.

7. The secondary battery according to claim 6, wherein C4 to C 10 The aliphatic trinitrile solvent is 1,3,6-hexanetrinitrile.

8. The secondary battery according to any one of claims 1 to 7, wherein the total amount of the polynitrile solvent contained in the electrolyte is an amount of 0.2 wt% to 50 wt%, preferably 2 wt% to 40 wt%, based on the total weight of the solvent composition. 9 . The secondary battery according to claim 1 , wherein the total amount of the polynitrile solvent contained in the electrolyte is in an amount of 1 wt % to 10 wt %, preferably 2 wt % to 5 wt %, based on the total weight of the solvent composition.

10. The secondary battery according to any one of claims 1 to 7, wherein the total amount of the polynitrile solvent contained in the electrolyte is an amount of 10 wt% to 50 wt%, preferably 20 wt% to 40 wt%, based on the total weight of the solvent composition. 11 . The secondary battery according to claim 1 , wherein the second solvent is a carbonate solvent.

12. The secondary battery according to any one of claims 1 to 11, wherein the carbonate solvent is dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, ethylmethyl carbonate, ethylmethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, or a combination thereof. 13 . The secondary battery according to claim 1 , wherein the carbonate solvent is ethylene carbonate, ethylmethyl carbonate, propylene carbonate, or a combination thereof. 14 . The secondary battery according to claim 13 , wherein the carbonate solvent comprises a mixture of ethylene carbonate and ethyl methyl carbonate or a mixture of propylene carbonate and ethyl methyl carbonate. 15 . The secondary battery according to claim 14 , wherein a weight ratio of the ethylene carbonate to the ethyl methyl carbonate or a weight ratio of the propylene carbonate to the ethyl methyl carbonate is 30:70 to 50:

50. 16 . The secondary battery according to claim 1 , wherein the carbonate solvent is propylene carbonate, and the total amount of propylene carbonate contained in the electrolyte is in an amount of at least 1 wt % based on the total weight of the solvent composition.

17. The secondary battery according to any one of claims 1 to 10, wherein the second solvent is an ester solvent, for example, wherein the ester solvent is methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, 5-decanoic acid lactone, γ-valerolactone, dl-mevalonolactone, γ-caprolactone or a combination thereof.

18. The secondary battery according to any one of claims 1 to 10, wherein the second solvent is an ether solvent, for example wherein the ether solvent is dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

19. The secondary battery according to any one of claims 1 to 10, wherein the second solvent is a mononitrile solvent, for example wherein the mononitrile solvent comprises a C2 to C8 aliphatic mononitrile. 20 . The secondary battery according to claim 19 , wherein the C2 to C8 aliphatic mononitrile comprises butyronitrile, acetonitrile, propionitrile, acetonitrile, or a combination thereof. 21 . The secondary battery according to claim 19 , wherein the total amount of C2 to C8 aliphatic mononitriles in the electrolyte is 30 to 90 wt % based on the total weight of the solvent composition. 22 . The secondary battery according to claim 1 , wherein the electrolyte further comprises a lithium salt.

23. The secondary battery according to claim 22, wherein the lithium salt comprises LiBF4, LiPF6, or lithium difluoro(oxalato)borate, preferably LiBF4 or LiPF6, more preferably LiBF4.

24. The secondary battery according to claim 22 or 23, wherein the total lithium ion concentration in the electrolyte is 0.5 to 3 mol / L.

25. The secondary battery according to any one of claims 22 to 24, wherein the electrolyte comprises 0.8 mol / L to 3 mol / L of LiPF6.

26. A secondary battery according to any one of claims 22 to 24, wherein the electrolyte contains less than 0.1 mol / L of PF6 - , preferably wherein the electrolyte does not contain PF6 - . 27 . The secondary battery according to claim 1 , wherein the negative electrode comprises niobium metal oxide.

28. The secondary battery according to any one of claims 1 to 27, wherein the niobium metal oxide is Nb 14 W3O 44 , Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 、Nb2Mo3O 14 , Nb 14 Mo3O 44 , Nb 12 MoO 44 or a combination thereof, preferably Nb 16 W5W 55 or Nb 18 W 16 O 93 or a combination thereof, more preferably Nb 16 W5W 55 .

29. A method for manufacturing a secondary battery, the method comprising: Provide positive electrode, providing a negative electrode comprising niobium oxide or niobium metal oxide, and providing a separator between the positive electrode and the negative electrode; as well as Providing an electrolyte comprising A solvent composition comprising: a polynitrile solvent having two or more nitrile groups, and at least one second solvent selected from the group consisting of a mononitrile solvent, a carbonate solvent, an ester solvent or an ether solvent, wherein the polynitrile is contained in an amount of at least 0.1 wt % based on the total weight of the solvent composition, and The cathode, the anode, and the separator are brought into contact with the electrolyte to manufacture the secondary battery.

30. The method of claim 29, wherein the electrolyte comprises a lithium salt.

31. The method according to claim 29 or 30, wherein the polynitrile solvent is a dinitrile solvent or a trinitrile solvent, preferably a dinitrile solvent.

32. The method of any one of claims 29 to 31, wherein the negative electrode comprises niobium metal oxide.