Preparation method of lithium hexafluorophosphate solution capable of reducing content of reaction by-products

By using purified organic solvents and fine reaction control, combined with membrane filtration and deacidification operations, the by-product and water sensitivity issues in lithium hexafluorophosphate solutions are solved, improving battery performance and life.

CN118791018AActive Publication Date: 2024-10-18FUJIAN QINGLIU DONGYING CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410786097.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

It is difficult to obtain high purity when preparing lithium hexafluorophosphate solution with the existing technology, and there are problems with reaction by-products and water sensitivity. It is also difficult to control the reaction conditions, which affects battery performance and life.

Method used

A mixed organic solvent of purified dimethyl carbonate and ethyl methyl carbonate is used, and the water is removed through molecular sieve drying and gas chromatography detection. The appropriate solvent ratio and reaction conditions are selected, combined with membrane filtration and deacidification operations to ensure high purity and stability.

Benefits of technology

It significantly reduces the content of reaction by-products, controls water sensitivity, ensures the high purity and battery performance of lithium hexafluorophosphate, and improves the service life and stability of the battery.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a lithium hexafluorophosphate solution capable of reducing the content of reaction byproducts, belongs to the technical field of lithium ion electrolyte manufacturing, and solves the problems that the content of the reaction byproducts is too high and impurities are not easy to remove in the existing preparation method. The method comprises the following steps: S1, preparing an organic solvent; s2, preparing purified phosphorus pentafluoride gas; s3, preparing a suspension mixture; s4, preparing a lithium hexafluorophosphate solution in an initial stage; s5, adsorbing impurities; s6, preliminary filtering; s7, carrying out deacidification; and S8, precisely filtering. According to the method, the lithium hexafluorophosphate solution with high purity and low impurity content is successfully prepared through high-purity preparation of raw materials, strict reaction control, effective impurity removal steps and application of a precise filtering technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion electrolyte manufacturing, and relates to a lithium hexafluorophosphate solution, in particular to a preparation method of a lithium hexafluorophosphate solution with reduced content of reaction by-products. Background Art

[0002] As a key material for lithium-ion batteries, lithium hexafluorophosphate is usually used in battery electrolytes by mixing with organic solvents to form liquid lithium salts. The organic solvent method has good controllability and can control the reaction process and product properties by adjusting the reaction conditions and solvent types to meet the needs of different applications. The organic solvent method can usually achieve a higher yield. However, there are still some challenges that need to be overcome:

[0003] High purity requirements: The lithium hexafluorophosphate used in battery electrolytes needs to have extremely high purity. When prepared using the organic solvent method, the reaction raw materials may undergo adverse reactions such as polymerization and decomposition with some organic solvents, resulting in the production of reaction by-products. It is difficult to obtain high-purity lithium hexafluorophosphate, which has a serious impact on the performance and life of the battery. It is not easy to reduce the production of reaction by-products and remove reaction by-products during the production process.

[0004] Water sensitivity: Lithium hexafluorophosphate is sensitive to water and easily absorbs water to form hydrates, thus affecting its performance in the electrolyte. Effectively controlling the introduction of water and preventing the formation of hydrates are issues that need to be addressed during the preparation process.

[0005] Reaction condition control: In the organic solvent method, changes in reaction conditions may lead to different side reaction pathways, thereby affecting the quality of the product. It is crucial to determine and accurately control the reaction conditions to ensure the consistency and purity of the product.

[0006] Unsatisfactory solvent performance: The performance of a single organic solvent is often not ideal, which will lead to poor performance of the battery during use. Therefore, when selecting an organic solvent, its performance needs to be comprehensively considered to improve the solubility and stability of lithium hexafluorophosphate.

[0007] Solving these difficulties is crucial to improving the preparation efficiency, product quality and battery performance of lithium hexafluorophosphate; with the widespread application of lithium-ion batteries in new energy vehicles and secondary batteries, how to solve these difficulties becomes extremely urgent and critical. Summary of the invention

[0008] The purpose of the present invention is to solve the above problems in the prior art and to provide a method for preparing a lithium hexafluorophosphate solution with reduced content of reaction by-products.

[0009] The object of the present invention can be achieved by the following technical scheme: A method for preparing a lithium hexafluorophosphate solution with reduced content of reaction by-products, the preparation method comprising the following steps:

[0010] S1 Preparation of organic solvent: Purification: purifying dimethyl carbonate and ethyl methyl carbonate respectively to obtain purified dimethyl carbonate and purified ethyl methyl carbonate; Mixing: mixing the purified dimethyl carbonate and purified ethyl methyl carbonate by a mixing device until uniform to obtain a solvent mixture; Drying: drying the solvent mixture by a molecular sieve drying method to obtain an organic solvent; the purity of the organic solvent is greater than 99.9%;

[0011] The purpose of purification treatment is as follows: dimethyl carbonate and ethyl methyl carbonate products purchased on the market contain more impurities. In the preparation of high-purity lithium hexafluorophosphate solution, the raw materials used need to be as pure as possible. The purification of dimethyl carbonate and ethyl methyl carbonate can remove potential impurities, such as moisture, other organic impurities or unreacted raw materials, which will affect the quality of the final product; improve reaction efficiency: purified solvents can improve the efficiency of chemical reactions, reduce the occurrence of side reactions, and thus reduce the generation of by-products; improve the purity of the final product: the use of high-purity solvents can directly affect the purity of the final product, which is particularly important for the battery industry.

[0012] The reasons for choosing a mixture of purified dimethyl carbonate and purified ethyl methyl carbonate as the organic solvent are as follows: Boiling point: The boiling point of dimethyl carbonate is about 90°C, while the boiling point of ethyl methyl carbonate is about 107°C, which means that they can evaporate at a lower temperature. The difference in boiling points between the two is conducive to controlling the evaporation and recovery of the solvent at different temperature stages; both are considered to be relatively safe and environmentally friendly solvents;

[0013] Functions and advantages of dimethyl carbonate: Good solubility: It has good lithium salt solubility, which helps to maintain the high solubility of lithium hexafluorophosphate in the electrolyte; High conductivity: The relatively high conductivity helps to improve the conductivity of the electrolyte, reduce the internal resistance of the battery, and thus improve the power performance of the battery; Low temperature performance: It can still maintain good performance in low temperature environments, so that the battery can work normally in cold areas; Improve battery energy density: The use of dimethyl carbonate helps to improve the energy density of the battery because it can provide relatively high capacity.

[0014] Functions and advantages of ethyl methyl carbonate: Solubility and stability: ethyl methyl carbonate has good lithium salt solubility, which helps to maintain the stability of the electrolyte. It can form a stable electrolyte membrane and improve the cycle life of the battery; Temperature adaptability: It performs relatively well at low temperatures, which helps to improve the performance of the battery in cold environments; Reduce the risk of crystallization: The use of ethyl methyl carbonate can reduce the risk of lithium hexafluorophosphate crystallization in the electrolyte, which helps to maintain the stability of the battery; Increase the viscosity of the electrolyte: ethyl methyl carbonate has a certain viscosity, which can increase the viscosity of the electrolyte and help prevent leakage problems in the battery.

[0015] Through reasonable mixing, the respective advantages of dimethyl carbonate and ethyl methyl carbonate can be fully utilized, while balancing their different characteristics to meet the requirements of battery design. Such mixed organic solvents help improve battery performance, safety and cycle life.

[0016] Reasons for choosing the ratio of 19.744-29.616:17.856-26.784: Balanced polarity and solubility: This ratio was determined through a large number of experiments in laboratory and industrial practice, and it balances the polarity and solubility of the solvent; the higher polarity of dimethyl carbonate combined with the stable solvent environment of ethyl methyl carbonate provides the best lithium salt dissolution effect; Thermal stability and evaporation control: This ratio takes into account both thermal stability and the evaporation characteristics of the solvent, and the volatilization and recovery of the solvent can be more effectively controlled; Optimizing reaction conditions: This ratio can optimize the conditions of the chemical reaction, reduce the possibility of side reactions and increase the yield of the target product.

[0017] The purpose of drying is to remove moisture because trace amounts of water will also undergo hydrolysis reaction with lithium hexafluorophosphate, so drying is performed to remove moisture.

[0018] S2 Preparation of purified phosphorus pentafluoride gas: Mixing: Mix phosphorus trichloride and fluorine gas in a corrosion-resistant reactor; Initiate a reaction under a controlled environment to obtain a mixed gas; Cool the mixed gas;

[0019] Preliminary purification: using alkaline solution to remove chlorine from the cooled mixed gas; fractional purification: using a fractionation tower for further purification to obtain purified phosphorus pentafluoride gas, which is collected using a gas collection device and stored in a low-temperature environment;

[0020] The purpose of preparing purified phosphorus pentafluoride gas is as follows: phosphorus pentafluoride is a key raw material for preparing lithium hexafluorophosphate; high-purity phosphorus pentafluoride is crucial to the quality of the final product. The phosphorus pentafluoride purchased on the market contains impure substances, such as P2O5, PF3 and other impurities, which are not conducive to the subsequent reactions. The high purity of phosphorus pentafluoride ensures the selectivity of the reaction and the purity of the product. The pure state of phosphorus pentafluoride helps to reduce side reactions and improve reaction efficiency.

[0021] S3 preparation of suspension mixture: adding an organic solvent to a reactor, conveying lithium fluoride to the reactor through a powder feeding device, and performing a first stirring with a stirring device to form a suspension mixture, wherein the reactor is equipped with a temperature control device and a pressure monitoring device; in the suspension mixture, the weight ratio of organic solvent to lithium fluoride is 5-10:1;

[0022] The reasons for selecting the organic solvent and lithium fluoride as 5-10:1 are as follows: Solubility of lithium hexafluorophosphate: The solubility of lithium hexafluorophosphate in organic solvent is the key. When phosphorus pentafluoride gas reacts with suspended lithium fluoride, the generated lithium hexafluorophosphate will form a dense protective film on the surface of lithium fluoride, which will hinder the reaction. The role of the organic solvent here is to quickly dissolve the generated lithium hexafluorophosphate, thereby breaking this protective film and ensuring that the reaction can continue and be as complete as possible; Reaction kinetics: The amount of organic solvent affects the kinetics of the entire reaction. In an appropriate proportion of organic solvent, the fluidity of the reaction mixture is better, which is conducive to effective contact between gas and solid and promotes the reaction; Preventing supersaturation and precipitation: Too high solid concentration may cause the solution to be supersaturated, causing lithium hexafluorophosphate to precipitate instead of dissolving; Maintaining a suitable ratio of organic solvent and lithium fluoride can ensure that lithium hexafluorophosphate is effectively dissolved instead of forming solid precipitation; Improving product quality: By controlling the amount of organic solvent, the concentration and quality of the generated lithium hexafluorophosphate solution can be controlled to a certain extent, avoiding the generation of impurities caused by incomplete reaction or supersaturation.

[0023] S4 Preparation of lithium hexafluorophosphate solution in the initial stage: Under normal pressure, purified phosphorus pentafluoride gas is introduced into the suspension mixture, and a stirring device is started for a second stirring, the stirring speed of the second stirring is 200-500rpm, the time for introducing purified phosphorus pentafluoride gas is the same as the time for the second stirring, and after the purified phosphorus pentafluoride gas introduction work is completed; a stirring device is used for a third stirring, and the stirring speed is 100-300rpm; when the pressure in the reactor is no longer changed by monitoring the pressure monitoring device, the third stirring operation is stopped to obtain the lithium hexafluorophosphate solution in the initial stage; purified phosphorus pentafluoride gas is introduced: lithium fluoride according to the molar ratio of 1.1-1.2:1; the residual purified phosphorus pentafluoride gas is sent to the tail gas treatment system and treated by water alkali washing method;

[0024] The reason for selecting the molar ratio of 1.1-1.2:1 is that a slightly excess of phosphorus pentafluoride gas can ensure that lithium fluoride is completely reacted to generate lithium hexafluorophosphate; at the same time, it can prevent the product purity from being low due to insufficient phosphorus pentafluoride gas.

[0025] S5: adsorbing impurities: adding a purifying agent to the lithium hexafluorophosphate solution in the initial stage, and performing a fourth stirring operation using a stirring device. After the fourth stirring operation is completed, the solution is allowed to stand to obtain a lithium hexafluorophosphate solution in the intermediate stage;

[0026] S6 preliminary filtration: the lithium hexafluorophosphate solution in the intermediate stage is subjected to preliminary filtration operation through a membrane filter device to obtain a filtered lithium hexafluorophosphate solution;

[0027] The reasons for using membrane filter equipment are: efficient separation ability: membrane filters can effectively separate suspended particles and larger molecular impurities in the solution through the principle of physical size exclusion, which is crucial to improving the purity of lithium hexafluorophosphate solution; easy operation: compared with traditional filtration methods, membrane filtration equipment is more efficient and easy to operate, suitable for continuous or batch production processes; controllable separation process: by selecting filter membranes with different pore sizes, the filtration effect can be precisely controlled to meet the specific purity requirements of lithium hexafluorophosphate solution.

[0028] S7 Deacidification: The filtered lithium hexafluorophosphate solution is deacidified to obtain a deacidified lithium hexafluorophosphate solution; the purpose of the deacidification operation is as follows: Improve product purity: As a key component of battery electrolyte, the purity of lithium hexafluorophosphate has a direct impact on the performance of the battery. The presence of acidic substances will reduce the purity of lithium hexafluorophosphate, thereby affecting the performance and life of the battery; Improve battery safety: Acidic substances may react with other components in the battery to produce harmful substances or gases, increasing safety risks during battery use; Prevent corrosion: Acidic substances may corrode materials inside the battery, such as electrodes and diaphragms, affecting the structural integrity and performance of the battery; Improve electrolyte stability: Acidic substances may accelerate the degradation of the electrolyte, reducing the cycle life and energy storage efficiency of the battery; Meet standard requirements: The battery manufacturing industry has strict standards for the purity of the electrolyte. Through the deacidification step, it can be ensured that the lithium hexafluorophosphate solution meets these standards.

[0029] S8 precision filtration: Use precision filtration equipment to perform precision filtration on the deacidified lithium hexafluorophosphate solution to obtain a lithium hexafluorophosphate solution. Precision filtration helps to improve the purity of the final product and ensure that the lithium hexafluorophosphate solution does not contain any unremoved tiny impurities.

[0030] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S1, the purification treatment is to perform a rectification operation on the pre-purified product through a distillation tower, and then collect the top product of the distillation tower, and use a gas chromatography method to detect the top product of the distillation tower during the purification process to meet the purity requirements;

[0031] After purification, the purity of purified dimethyl carbonate is greater than 99.9%; the purity of purified ethyl methyl carbonate is greater than 99.9%;

[0032] In the dimethyl carbonate purification process, the distillation temperature is 90-120° C. and the distillation pressure is 1-1.5 atmospheres; in the ethyl methyl carbonate purification process, the distillation temperature is 107-135° C. and the distillation pressure is 1-1.5 atmospheres; the distillation temperature and pressure are selected to obtain the best separation effect within the effective energy consumption, and these parameters are determined based on the boiling point, vapor pressure and chemical stability of dimethyl carbonate and ethyl methyl carbonate; these temperature and pressure parameters are high enough to achieve effective distillation and can effectively avoid thermal decomposition or unnecessary chemical reactions.

[0033] During the drying operation, the drying temperature is 40-60°C and the drying duration is 6-12 hours; the moisture content of the organic solvent is detected by the Karl Fischer moisture determination method, and the moisture content in the organic solvent is not higher than 35ppm; the molecular sieve type is one of 3A, 4A and 5A molecular sieves; the pore size of 3A, 4A and 5A molecular sieves can effectively adsorb and remove moisture and other small molecular impurities in the solvent, while avoiding the adsorption of large molecules, which helps to maintain the chemical structure and purity of the solvent.

[0034] Steps for gas chromatography to detect the top product of the fractionator: Sampling: Collect samples from the top of the fractionator;

[0035] Injection: injecting the sample into the gas chromatography device; separation: the sample is separated according to molecular characteristics in the chromatographic column; detection: quantitative analysis of each component through the detector; data analysis: comparing the chromatogram peaks with known standard substances to determine the purity of the components.

[0036] The steps for Karl Fischer moisture determination to detect moisture content are as follows: Prepare samples: prepare samples and ensure that the properties and state of the samples are suitable for Karl Fischer determination; Solvent preparation: prepare appropriate Karl Fischer solvents, using methanol or isopropanol as solvents, which contain Karl Fischer reagents; Calibration: before starting the actual measurement, calibrate the instrument; including calibrating electrodes and magnetic stirrers; Pre-determination: take a certain amount of sample and put it into the instrument, and pass dry nitrogen to remove moisture from the sample; Start titration: Start the Karl Fischer titrator and titrate the Karl Fischer reagent into the sample. The Karl Fischer reagent will react with water to generate hydrogen. This titration process will be automatically monitored by the instrument; End point detection: when the moisture in the sample is completely reacted, the titration will terminate. The end point detection is completed by detecting the change in electrode potential or current; Calculate moisture content: the moisture content in the sample can be calculated by the known concentration of Karl Fischer reagent and the volume of Karl Fischer reagent used in the titration process.

[0037] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S2, the molar ratio of phosphorus trichloride to fluorine gas is 1:5; the controlled environment includes controlling the reaction temperature to 200-300° C. and the reaction pressure to 2-5 atmospheres;

[0038] Cooling temperature is -40℃-0℃;

[0039] The alkaline solution is any one of a sodium hydroxide solution, a potassium hydroxide solution and aqueous ammonia, wherein the concentration of the sodium hydroxide solution is 15% to 30%, the concentration of the potassium hydroxide solution is 15% to 30%, and the concentration of the aqueous ammonia is 25%-30%;

[0040] During the fractionation and purification process, the operating temperature in the fractionation tower is controlled to be -85.5°C--75.5°C, the operating pressure of the fractionation tower is 0.6-0.9 atmospheres, and the number of layers of the fractionation tower is 10-20. During the fractionation operation, gas chromatography is used for purity detection to ensure that the purity of the purified phosphorus fluoride gas reaches more than 99.9%.

[0041] Temperature has a significant impact on the synthesis of phosphorus pentafluoride. At a temperature of 200-300°C, the reaction between phosphorus trichloride and fluorine gas tends to be complete. If the temperature is too low, the reaction is incomplete and the yield is low. If the temperature is too high, it will cause unnecessary side reactions and equipment damage.

[0042] Controlling the pressure at 2-5 atmospheres is beneficial to maintaining the stability of the reaction and increasing the reaction rate; too high a pressure may cause equipment pressure over-limit and safety risks, while too low a pressure may result in insufficient reaction.

[0043] Cooling temperature is -40℃-0℃; cooling is to condense the generated phosphorus pentafluoride gas to facilitate subsequent purification treatment. This temperature range can effectively condense phosphorus pentafluoride while avoiding the condensation of other low-boiling impurities.

[0044] Temperature control during the fractionation process is critical, and the temperature range of -85.5°C to -75.5°C is optimized based on the boiling point of phosphorus pentafluoride gas and the boiling points of possible impurities.

[0045] Working pressure 0.6-0.9 atmosphere: Distillation at a lower pressure helps to improve separation efficiency and reduce energy consumption. This pressure range is suitable for the effective distillation of phosphorus pentafluoride while also ensuring the safe operation of the equipment.

[0046] The number of layers of the distillation tower is 10-20: The number of layers of the distillation tower affects the efficiency and purity of the distillation. 10-20 layers can improve the separation efficiency while controlling the size and cost of the equipment.

[0047] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced content of reaction by-products, in step S3, in one stirring operation, the working temperature of the temperature control device is set to 10-15°C, and the working pressure of the pressure monitoring device is set to 1-2 atmospheres; the stirring speed is 100-300rpm; the stirring time is 30-60 minutes; during the first stirring process, sampling and detection using a suspension particle size analyzer are performed to ensure that the suspension mixture is uniform.

[0048] The stirring speed is 100-300 rpm: This speed range helps to ensure uniform mixing of the suspension and avoid particle breakage or excessive shear force caused by too fast stirring;

[0049] How to use the suspension particle size analyzer:

[0050] Sample preparation: Take a representative sample from the reactor;

[0051] Equipment calibration: Ensure that the suspension particle size analyzer is accurately calibrated to obtain reliable data;

[0052] Sample loading: placing the sample in the sample chamber of the analyzer;

[0053] Test run: Start the equipment and perform particle size analysis.

[0054] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S4, the operating temperature of the temperature control device is set to 10-15° C.; the introduction rate of the purified phosphorus pentafluoride gas is 0.05-0.2 L / min.

[0055] The purpose of temperature control: Under low temperature conditions of 10-15°C, the reaction rate can be slowed down to avoid heat accumulation and side reactions caused by too fast reaction; The effect of temperature on product quality: Low temperature helps to improve the purity and quality of lithium hexafluorophosphate and reduce the generation of by-products;

[0056] The introduction rate of 0.05-0.2 L / min is based on the consideration of ensuring sufficient reaction between gas and solid. Too fast an introduction rate may lead to difficulty in reaction control, while too slow an introduction rate may reduce production efficiency.

[0057] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S5, the stirring speed of the four stirring operations is 150-300 rpm, the stirring time is 20-40 minutes, the standing time is 1-2 hours, and the purifier is succinic acid exchange resin; the amount of the succinic acid exchange resin is 5-10 grams per liter of lithium hexafluorophosphate solution in the initial stage.

[0058] Succinic acid exchange resin has good chemical stability and will not react with other components of the solution, thus ensuring the stability and reliability of the adsorption effect; succinic acid exchange resin has high adsorption capacity and can effectively remove impurities in lithium hexafluorophosphate solution, such as unreacted raw materials or by-products; the use of succinic acid exchange resin for adsorption is simple, and the resin can be reused through a regeneration process, thus improving the economic benefits of the entire process.

[0059] Adsorption capacity: The adsorption capacity of succinic acid exchange resin is limited. The amount of 5-10 grams per liter of lithium hexafluorophosphate solution used in the initial stage is determined based on experiments and production practice, which can ensure that impurities are effectively removed.

[0060] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S6, the preliminary filtration step is as follows:

[0061] B1 transferring the lithium hexafluorophosphate solution in the intermediate stage from the reactor to the membrane filter device, the working flow rate of the membrane filter device is 0.5-1 liter / minute, and the working pressure of the membrane filter device is 1.5-3 atmospheres;

[0062] B2 uses a filter membrane with a pore size of 5-10 microns for the first stage of filtration;

[0063] B3 uses a filter membrane with a pore size of 0.45-1 micron for the second stage of filtration;

[0064] B4 monitors the pressure and flow rate during the filtration process to ensure filtration efficiency.

[0065] The working flow rate of the membrane filter equipment is 0.5-1 liter / minute: This flow rate range is based on the balance between obtaining the best filtration effect and maintaining high processing efficiency. Too fast a flow rate may lead to reduced filtration efficiency, while too slow a flow rate reduces production efficiency. Controlling the appropriate flow rate helps prevent membrane clogging and damage and extend the service life of the membrane.

[0066] The working pressure of membrane filter equipment is 1.5-3 atmospheres: this pressure range ensures that the solution passes through the filter membrane effectively while avoiding excessive mechanical pressure on the membrane and reducing the risk of membrane wear and damage; appropriate working pressure is essential to maintaining filtration efficiency and quality. Excessive pressure may cause membrane rupture or excessive material penetration, while too low pressure may result in insufficient treatment efficiency.

[0067] Selection of pore size, 5-10 microns in the first stage and 0.45-1 microns in the second stage: By using filter membranes with different pore sizes in stages, impurities of different sizes can be removed more effectively, with larger particles removed in the first stage and further refined in the second stage; such a combination of pore sizes helps to balance filtration efficiency and purity requirements, ensuring that the final product meets high quality standards.

[0068] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content, in step S7, the deacidification operation steps are as follows:

[0069] C1 Deacidification environment setting: Ensure that the entire deacidification process is carried out under a nitrogen atmosphere to exclude interference from air and moisture;

[0070] C2 deacidification agent addition: the deacidification agent is added in a stepwise manner to neutralize and filter the acidic substances in the lithium hexafluorophosphate solution, wherein the deacidification agent is any one of anhydrous sodium hydroxide and anhydrous sodium carbonate; during the addition of the deacidification agent, the concentration of the acidic substances in the deacidified lithium hexafluorophosphate solution is detected by an ion chromatograph to ensure that the acidic substances are completely neutralized.

[0071] The steps for using an ion chromatograph to detect the concentration of acidic substances are as follows: Sampling: At different stages of adding the deacidifying agent, a small amount of samples are periodically taken out from the reaction system; Sample processing: The samples are appropriately diluted to meet the detection requirements of the ion chromatograph; Chromatographic analysis: Use an ion chromatograph to analyze and determine the concentration of acidic substances in the solution; Result evaluation: Evaluate the removal of acidic substances based on the chromatographic analysis results to guide whether further addition of deacidifying agents is needed; Repeat detection: During the entire deacidification process, repeat sampling and analysis as needed until it is confirmed that all acidic substances have been completely neutralized.

[0072] In the above-mentioned method for preparing a lithium hexafluorophosphate solution with a reduced content of reaction by-products, in step S8, the precision filtration equipment includes: a feed pump: used to transport the solution to be filtered to the filtration system; a pre-filter: used to remove larger particles in the solution; a main filter, including a precision microporous filter membrane and a deep filter material; a flow meter and a pressure gauge: used to monitor the flow rate and pressure during the filtration process in real time to ensure that the equipment operates in an optimal state; a filtration control system: used to adjust the filtration speed and filtration pressure to ensure filtration efficiency and product quality;

[0073] The steps for fine filtering the deacidified lithium hexafluorophosphate solution are as follows:

[0074] D1 Preparation stage: Ensure that the precision filtration equipment is in a clean state to avoid the introduction of new impurities; perform integrity tests on the pre-filter and main filter to ensure that there is no damage or leakage;

[0075] D2 filter start: start the feed pump to slowly deliver the deacidified lithium hexafluorophosphate solution to the pre-filter; in the pre-filtration stage, particles larger than 10 microns are removed; adjust the flow rate and pressure to ensure that the solution passes through the pre-filter smoothly, the flow rate is controlled at 0.1-0.5 liters / minute, and the filtration pressure is 0.2-0.5 atmospheres;

[0076] D3 main filtration process: the solution after pre-filtration first passes through the precision microporous filter membrane to remove fine particles in the solution. The flow rate of the solution through the precision microporous filter membrane is 0.05-0.2 liters / minute, and the filtration pressure is 0.5-1.5 atmospheres; the pore size of the precision microporous filter membrane is 4-10 microns;

[0077] The solution filtered through the precision microporous filter membrane then flows through the deep filter material, which is composed of porous, highly adsorbent ion exchange resin to capture smaller particles and soluble impurities; the number of layers of the deep filter material is 3-6; the pore size range of the deep filter material gradually transitions from 1-5 microns to 0.1-1 microns; the flow rate and pressure in the main filtration process are monitored in real time by flow meters and pressure gauges;

[0078] D4 filtration test: Take samples regularly and use atomic absorption spectroscopy to check the purity of the solution. If the test fails, adjust the filtration speed and pressure through the filtration control system; or replace the precision microporous filter membrane and deep filtration material.

[0079] The flow rate in the pre-filtration stage is controlled at 0.1-0.5 L / min and the pressure is 0.2-0.5 atmospheres: the purpose of this stage is to remove larger particles. The appropriate flow rate and pressure can ensure that the solution passes through the filter smoothly and avoid damage to the filter membrane or loss of efficiency due to excessive flow rate or pressure.

[0080] The flow rate of the precision microporous filter membrane is controlled at 0.05-0.2 liters / minute and the pressure is 0.5-1.5 atmospheres: at this stage, fine particles are removed; lower flow rates are conducive to improving filtration efficiency, allowing more particles to be captured by the filter membrane; at the same time, appropriate pressure ensures that the solution can effectively pass through the filter membrane without causing clogging.

[0081] The pore size of the precision microporous filter membrane is 4-10 microns: this pore size can effectively remove fine particles in the solution while preventing the filter membrane from clogging too quickly.

[0082] The pore size range of the depth filter material gradually transitions from 1-5 microns to 0.1-1 microns: this progressive pore size setting helps capture particles of different sizes in stages, thereby improving filtration efficiency and purity; the large pore size layer captures larger particles first, while the finer pore size is responsible for removing smaller particles.

[0083] Porous, highly adsorptive ion exchange resins: These materials are chosen because they can effectively capture tiny particles and dissolved impurities in the solution. The porous structure of ion exchange resins provides a large amount of surface area, making them highly efficient adsorbents. In addition, these resins are selective and adsorbent for specific ions such as metal ions and other contaminants, which helps to further improve the purity of the solution.

[0084] Compared with the prior art, the present invention has the following beneficial effects:

[0085] 1. Reduction of the content of reaction by-products: By preparing and purifying pentafluoride and purified organic solvents, high-purity raw materials are provided, and by selecting a suitable organic solvent ratio, the content of reaction by-products is effectively reduced through precise control of reaction conditions, the purity of lithium hexafluorophosphate is improved, and the problem of difficulty in obtaining high-purity products during the preparation process is solved.

[0086] 2. Water sensitivity control: This preparation method effectively controls the introduction of water, which helps prevent lithium hexafluorophosphate from absorbing water to form hydrates, thereby maintaining its performance in the electrolyte.

[0087] 3. Precise control of reaction conditions: By monitoring temperature, stirring and pressure at different stages of the preparation process, accurate control of reaction conditions can be ensured, which helps to avoid the occurrence of different side reaction pathways, ensure the consistency and purity of the products, and solve the challenges in controlling reaction conditions.

[0088] 4. Optimization of organic solvent performance: Comprehensive consideration has been given to the selection and ratio of organic solvents to improve the solubility and stability of lithium hexafluorophosphate, which helps to solve the problem of unsatisfactory performance of a single organic solvent and improve the effect of the battery during use.

[0089] 5. Staged filtration and deacidification operations: By introducing purifiers, preliminary filtration, deacidification and other operations during the preparation process, reaction by-products and other impurities can be effectively removed, which helps to obtain high-quality lithium hexafluorophosphate solution.

[0090] In summary, the present invention improves the preparation efficiency of lithium hexafluorophosphate and the purity of the product, solves the problems of water sensitivity and reaction condition control, and improves the performance and life of the battery. DETAILED DESCRIPTION

[0091] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0092] A method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content comprises the following steps:

[0093] S1. Preparation of organic solvent: purification treatment: purifying dimethyl carbonate and ethyl methyl carbonate respectively to obtain purified dimethyl carbonate and purified ethyl methyl carbonate;

[0094] Mixing: Purified dimethyl carbonate and purified ethyl methyl carbonate are mixed uniformly by a mixing device to obtain a solvent mixture; in the solvent mixture, the weight ratio of purified dimethyl carbonate to purified ethyl methyl carbonate is 19.744:17.856;

[0095] Drying: The solvent mixture is dried by molecular sieve drying to obtain an organic solvent; the purity of the organic solvent is greater than 99.9%;

[0096] The purification process is to perform a rectification operation on the pre-purified product through a distillation tower, and then collect the top product of the distillation tower. During the purification process, the top product of the distillation tower is detected by gas chromatography to meet the purity requirements;

[0097] After purification, the purity of purified dimethyl carbonate is greater than 99.9%; the purity of purified ethyl methyl carbonate is greater than 99.9%;

[0098] In the process of purifying dimethyl carbonate, the distillation temperature is 90-120°C and the distillation pressure is 1-1.5 atmospheres; in the process of purifying ethyl methyl carbonate, the distillation temperature is 107-135°C and the distillation pressure is 1-1.5 atmospheres;

[0099] In the drying operation, the drying temperature is 40-60°C and the drying duration is 8 hours. The moisture content of the organic solvent is tested by Karl Fischer moisture determination method, and the moisture content in the organic solvent is 25ppm. The molecular sieve type is 4A molecular sieve.

[0100] S2 Preparation of purified phosphorus pentafluoride gas: Mixing: Mix phosphorus trichloride and fluorine gas in a corrosion-resistant reactor; Initiate a reaction under a controlled environment to obtain a mixed gas; Cool the mixed gas;

[0101] Initial purification: using alkaline solution to remove reaction byproducts from the cooled mixed gas;

[0102] Fractionation purification: further purification is performed using a fractionation tower to obtain purified phosphorus pentafluoride gas, which is collected using a gas collection device and stored in a low-temperature environment;

[0103] According to the molar ratio, phosphorus trichloride: fluorine gas is 1:5; the controlled environment includes controlling the reaction temperature to 200-300°C, controlling the reaction pressure to 2-5 atmospheres; the cooling temperature is -40°C-0°C;

[0104] The alkaline solution is 20% sodium hydroxide solution;

[0105] During the fractionation and purification process, the operating temperature of the distillation tower is controlled to be -85.5°C--75.5°C, the operating pressure of the distillation tower is 0.6-0.9 atmospheres, the number of layers of the distillation tower is 15, and during the fractionation operation, gas chromatography is used for purity detection, and the purity of the purified phosphorus pentafluoride gas reaches more than 99.9%.

[0106] S3 Preparation of suspended mixture: add organic solvent to the reactor, transport lithium fluoride to the reactor through powder feeding equipment, use stirring equipment to perform the first stirring to form a suspended mixture, the reactor is equipped with a temperature control device and a pressure monitoring device; in the suspended mixture, the weight ratio of organic solvent to lithium fluoride is 7:1; in the first stirring operation, set the working temperature of the temperature control device to 10-15°C, set the working pressure of the pressure monitoring device to 1-2 atmospheres; the stirring speed is 100-300rpm; the stirring time is 30-60 minutes,

[0107] S4 Preparation of lithium hexafluorophosphate solution in the initial stage: under normal pressure, purified phosphorus pentafluoride gas is introduced into the suspension mixture, and a stirring device is started for a second stirring, the stirring speed of the second stirring is 200-500rpm, the time for introducing purified phosphorus pentafluoride gas is the same as the time for the second stirring, and after the purified phosphorus pentafluoride gas is introduced; a stirring device is used for a third stirring at a stirring speed of 100-300rpm; when the pressure in the reactor is no longer changed by monitoring the pressure monitoring device, the third stirring operation is stopped to obtain a lithium hexafluorophosphate solution in the initial stage; purified phosphorus pentafluoride gas is introduced according to a molar ratio of 1.15:1 to lithium fluoride; the residual purified phosphorus pentafluoride gas is sent to the tail gas treatment system for treatment by water alkali washing method; the working temperature of the temperature control device is set to 10-15°C; the introduction rate of purified phosphorus pentafluoride gas is 0.05-0.2 liters / minute;

[0108] S5 adsorption of impurities: adding a purifier to the lithium hexafluorophosphate solution in the initial stage;

[0109] S6 Preliminary filtration: The lithium hexafluorophosphate solution in the intermediate stage is subjected to a preliminary filtration operation through a membrane filter device to obtain a filtered lithium hexafluorophosphate solution; the preliminary filtration steps are as follows:

[0110] B1 transferring the lithium hexafluorophosphate solution in the intermediate stage from the reactor to the membrane filter device, the working flow rate of the membrane filter device is 0.5-1 liter / minute, and the working pressure of the membrane filter device is 1.5-2 atmospheres;

[0111] B2 uses a filter membrane with a pore size of 8 microns for the first stage of filtration;

[0112] B3 uses a filter membrane with a pore size of 0.7 microns for the second stage of filtration;

[0113] B4 monitors the pressure and flow rate during the filtration process to ensure filtration efficiency.

[0114] S7 deacidification: performing a deacidification operation on the filtered lithium hexafluorophosphate solution to obtain a deacidified lithium hexafluorophosphate solution; the deacidification operation steps are as follows: C1 deacidification environment setting: ensuring that the entire deacidification process is carried out under a nitrogen atmosphere to exclude interference from air and moisture;

[0115] C2 deacidification agent addition: the deacidification agent is added in a stepwise manner to neutralize and filter the acidic substances in the lithium hexafluorophosphate solution, and the deacidification agent is anhydrous sodium hydroxide;

[0116] S8 precision filtration: Use precision filtration equipment to perform precision filtration on the deacidified lithium hexafluorophosphate solution to obtain a lithium hexafluorophosphate solution. The steps for precision filtration of the deacidified lithium hexafluorophosphate solution are as follows:

[0117] D1 Preparation stage: Ensure that the precision filtration equipment is in a clean state to avoid the introduction of new impurities; perform integrity tests on the pre-filter and main filter to ensure that there is no damage or leakage;

[0118] D2 filter start: start the feed pump to slowly deliver the deacidified lithium hexafluorophosphate solution to the pre-filter; in the pre-filtration stage, particles larger than 10 microns are removed; adjust the flow rate and pressure to ensure that the solution passes through the pre-filter smoothly, the flow rate is controlled at 0.1-0.3 liters / minute, and the filtration pressure is 0.2-0.5 atmospheres;

[0119] D3 main filtration process: the solution after pre-filtration first passes through the precision microporous filter membrane to remove fine particles in the solution. The flow rate of the solution through the precision microporous filter membrane is 0.05-0.2 liters / minute, and the filtration pressure is 0.5-1.5 atmospheres; the pore size of the precision microporous filter membrane is 4-10 microns;

[0120] The solution filtered through the precision microporous filter membrane then flows through the deep filter material, which is composed of porous, highly adsorbent ion exchange resin to capture smaller particles and soluble impurities; the number of layers of the deep filter material is 5; the pore size range of the deep filter material gradually transitions from 5 microns to 0.2 microns; the flow rate and pressure in the main filtration process are monitored in real time by flow meters and pressure gauges.

[0121] Purity test: The prepared lithium hexafluorophosphate solution is tested for purity using atomic absorption spectroscopy, the steps are as follows:

[0122] 1. Sample preparation: Take a sample from the prepared lithium hexafluorophosphate solution, ensure that no external impurities are introduced during the sampling process, and place the obtained sample in an appropriate container for further spectral analysis.

[0123] 2. Instrument calibration: Calibration is performed on the atomic absorption spectrometer to ensure that the instrument has an accurate understanding of the absorption characteristics of the target element. Calibration is performed using standards to establish a baseline for the absorption spectrum.

[0124] 3. Sample injection: gradually inject the obtained sample solution into the injection pool of the atomic absorption spectrometer; control the injection volume to ensure that the analysis is within the range specified by the instrument.

[0125] 4. Spectral scanning: Start the atomic absorption spectrometer for spectral scanning and record the absorption spectrum curve, including the position and intensity of the absorption peak.

[0126] 5. Data analysis: Use instrument software or related analysis tools to analyze the recorded spectral data.

[0127] 6. Confirm the elements in the solution and calculate their concentrations: Quality control: Perform quality control steps to check the signal-to-noise ratio, peak shape, peak width and other parameters of the spectrum; Result interpretation: Evaluate the purity of the lithium hexafluorophosphate solution based on the results of the spectral analysis; Detect the presence of different elements or impurities, as well as their concentrations.

[0128] After testing: in the lithium hexafluorophosphate solution, the content of reaction by-products is 0.0023%, the water content is: 0.0036%, the inorganic impurity Na+: 0.001%; ​​phosphorus pentafluoride: 0.001%.

[0129] The following conclusions were drawn from the analysis of the above data:

[0130] 1. Use of high-purity raw materials: In steps S1 and S2, by using organic solvents (dimethyl carbonate and ethyl methyl carbonate) with a purity exceeding 99.9% and phosphorus pentafluoride gas, the initial content of impurities is greatly reduced, which lays a solid foundation for the production of high-purity lithium hexafluorophosphate solution.

[0131] 2. Accurate reaction control: The temperature and pressure control (10-15°C, 1-2 atmospheres) and the strict setting of the stirring speed (100-300rpm) in step S3 ensure the uniformity and stability of the reaction, thereby reducing the occurrence of side reactions.

[0132] 3. In step S4, by controlling the introduction rate (0.05-0.2 L / min) and molar ratio (1.15:1) of phosphorus pentafluoride gas, the reaction efficiency is further optimized and the generation of by-products is reduced.

[0133] 4. Efficient impurity removal: The adsorption of impurities and preliminary filtration in steps S5 and S6 use filter membranes with specific pore sizes (first 8 microns and then 0.7 microns) to effectively remove larger particles and some fine impurities.

[0134] The deacidification process of S7 was carried out under a nitrogen atmosphere, which effectively eliminated the interference of air and moisture and further reduced the acidic substances in the solution.

[0135] 5. Precision filtration technology: The precision filtration equipment in step S8 effectively removes tiny particles and soluble impurities in the solution through multi-stage deep filtration, ensuring the high purity of the final product.

[0136] 6. Significant impurity reduction effect: After testing, the content of reaction by-products in lithium hexafluorophosphate solution.

Claims

1. A method for preparing a lithium hexafluorophosphate solution with reduced content of reaction by-products, characterized in that: The preparation method comprises the following steps: S1 organic solvent preparation: Purification treatment: purifying dimethyl carbonate and ethyl methyl carbonate respectively to obtain purified dimethyl carbonate and purified ethyl methyl carbonate; Mixing: Purified dimethyl carbonate and purified ethyl methyl carbonate are mixed uniformly by a mixing device to obtain a solvent mixture; in the solvent mixture, the weight ratio of purified dimethyl carbonate: purified ethyl methyl carbonate is 19.744-29.616:17.856-26.784; Drying: drying the solvent mixture by molecular sieve drying to obtain an organic solvent; the purity of the organic solvent is greater than 99.9%; S2 purified phosphorus pentafluoride gas preparation: Mixing: mixing phosphorus trichloride and fluorine gas in a corrosion-resistant reactor; initiating a reaction under a controlled environment to obtain a mixed gas; cooling the mixed gas; Initial purification: using alkaline solution to remove reaction byproducts from the cooled mixed gas; Fractionation purification: further purification is performed using a fractionation tower to obtain purified phosphorus pentafluoride gas, which is collected using a gas collection device and stored in a low-temperature environment; S3 preparation of suspension mixture: adding an organic solvent to a reactor, conveying lithium fluoride to the reactor through a powder feeding device, and performing a first stirring with a stirring device to form a suspension mixture, wherein the reactor is equipped with a temperature control device and a pressure monitoring device; in the suspension mixture, the weight ratio of organic solvent to lithium fluoride is 5-10:1; S4 Preparation of lithium hexafluorophosphate solution in the initial stage: Under normal pressure, purified phosphorus pentafluoride gas is introduced into the suspension mixture, and a stirring device is started for a second stirring, the stirring speed of the second stirring is 200-500rpm, the time for introducing purified phosphorus pentafluoride gas is the same as the time for the second stirring, and after the purified phosphorus pentafluoride gas introduction work is completed; a stirring device is used for a third stirring, and the stirring speed is 100-300rpm; when the pressure in the reactor is no longer changed by monitoring the pressure monitoring device, the third stirring operation is stopped to obtain the lithium hexafluorophosphate solution in the initial stage; purified phosphorus pentafluoride gas is introduced: lithium fluoride according to the molar ratio of 1.1-1.2:1; the residual purified phosphorus pentafluoride gas is sent to the tail gas treatment system and treated by water alkali washing method; S5: adsorbing impurities: adding a purifying agent to the lithium hexafluorophosphate solution in the initial stage, and performing a fourth stirring operation using a stirring device. After the fourth stirring operation is completed, the solution is allowed to stand to obtain a lithium hexafluorophosphate solution in the intermediate stage; S6 preliminary filtration: the lithium hexafluorophosphate solution in the intermediate stage is subjected to preliminary filtration operation through a membrane filter device to obtain a filtered lithium hexafluorophosphate solution; S7 deacidification: performing a deacidification operation on the filtered lithium hexafluorophosphate solution to obtain a deacidified lithium hexafluorophosphate solution; S8 precision filtration: Use precision filtration equipment to perform precision filtration operation on the deacidified lithium hexafluorophosphate solution to obtain a lithium hexafluorophosphate solution.

2. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S1, the purification process is to perform a rectification operation on the pre-purified product through a distillation tower, and then collect the top product of the distillation tower. During the purification process, the top product of the distillation tower is detected by gas chromatography to meet the purity requirements; After purification, the purity of purified dimethyl carbonate is greater than 99.9%; the purity of purified ethyl methyl carbonate is greater than 99.9%; In the process of purifying dimethyl carbonate, the distillation temperature is 90-120°C and the distillation pressure is 1-1.5 atmospheres; in the process of purifying ethyl methyl carbonate, the distillation temperature is 107-135°C and the distillation pressure is 1-1.5 atmospheres; During the drying operation, the drying temperature is 40-60°C and the drying duration is 6-12 hours. The moisture content of the organic solvent is tested by Karl Fischer moisture determination method, and the moisture content in the organic solvent is not higher than 35ppm. The molecular sieve type is one of 3A, 4A and 5A molecular sieves.

3. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S2, the molar ratio of phosphorus trichloride to fluorine gas is 1:5; the environment is controlled including controlling the reaction temperature to 200-300°C, controlling the reaction pressure to 2-5 atmospheres; the cooling temperature is -40°C-0°C; The alkaline solution is any one of a sodium hydroxide solution, a potassium hydroxide solution and aqueous ammonia, wherein the concentration of the sodium hydroxide solution is 15% to 30%, the concentration of the potassium hydroxide solution is 15% to 30%, and the concentration of the aqueous ammonia is 25%-30%; During the fractionation and purification process, the operating temperature of the distillation tower is controlled to be -85.5°C--75.5°C, the operating pressure of the distillation tower is 0.6-0.9 atmospheres, and the number of layers of the distillation tower is 10-20. During the fractionation operation, gas chromatography is used for purity detection to ensure that the purity of the purified phosphorus pentafluoride gas reaches more than 99.9%.

4. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S3, in the first stirring operation, the working temperature of the temperature control device is set to 10-15°C, and the working pressure of the pressure monitoring device is set to 1-2 atmospheres; the stirring speed is 100-300rpm; the stirring time is 30-60 minutes. During the first stirring process, sampling and testing with a suspension particle size analyzer are performed to ensure that the suspended mixture is uniform.

5. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S4, the operating temperature of the temperature control device is set to 10-15° C.; the introduction rate of the purified phosphorus pentafluoride gas is 0.05-0.2 liters / minute.

6. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S5, the stirring speed of the fourth stirring operation is 150-300 rpm, the stirring time is 20-40 minutes, the standing time is 1-2 hours, and the purifier is succinic acid exchange resin; the amount of the succinic acid exchange resin is 5-10 grams per liter of lithium hexafluorophosphate solution in the initial stage.

7. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S6, the preliminary filtering steps are as follows: B1 transferring the lithium hexafluorophosphate solution in the intermediate stage from the reactor to the membrane filter device, the working flow rate of the membrane filter device is 0.5-1 liter / minute, and the working pressure of the membrane filter device is 1.5-3 atmospheres; B2 uses a filter membrane with a pore size of 5-10 microns for the first stage of filtration; B3 uses a filter membrane with a pore size of 0.45-1 micron for the second stage of filtration; B4 monitors the pressure and flow rate during the filtration process to ensure filtration efficiency.

8. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S7, the deacidification operation steps are as follows: C1 Deacidification environment setting: Ensure that the entire deacidification process is carried out under a nitrogen atmosphere to exclude interference from air and moisture; C2 deacidification agent addition: the deacidification agent is added in a stepwise manner to neutralize and filter the acidic substances in the lithium hexafluorophosphate solution, wherein the deacidification agent is any one of anhydrous sodium hydroxide and anhydrous sodium carbonate; during the addition of the deacidification agent, the concentration of the acidic substances in the deacidified lithium hexafluorophosphate solution is detected by an ion chromatograph to ensure that the acidic substances are completely neutralized.

9. The method for preparing a lithium hexafluorophosphate solution with reduced reaction by-product content as claimed in claim 1, characterized in that: In step S8, the precision filtration equipment includes: a feed pump: used to deliver the solution to be filtered to the filtration system; a pre-filter: used to remove larger particles in the solution; a main filter, including a precision microporous filter membrane and a deep filter material; a flow meter and a pressure gauge: used to monitor the flow rate and pressure during the filtration process in real time to ensure that the equipment operates in the optimal state; a filtration control system: used to adjust the filtration speed and filtration pressure to ensure filtration efficiency and product quality; The steps for fine filtering the deacidified lithium hexafluorophosphate solution are as follows: D1 Preparation stage: Ensure that the precision filtration equipment is in a clean state to avoid the introduction of new impurities; perform integrity tests on the pre-filter and main filter to ensure that there is no damage or leakage; D2 filter start: start the feed pump to slowly deliver the deacidified lithium hexafluorophosphate solution to the pre-filter; in the pre-filtration stage, particles larger than 10 microns are removed; adjust the flow rate and pressure to ensure that the solution passes through the pre-filter smoothly, the flow rate is controlled at 0.1-0.5 liters / minute, and the filtration pressure is 0.2-0.5 atmospheres; D3 main filtration process: the solution after pre-filtration first passes through the precision microporous filter membrane to remove fine particles in the solution. The flow rate of the solution through the precision microporous filter membrane is 0.05-0.2 liters / minute, and the filtration pressure is 0.5-1.5 atmospheres; the pore size of the precision microporous filter membrane is 4-10 microns; The solution filtered through the precision microporous filter membrane then flows through the deep filter material, which is composed of porous, highly adsorbent ion exchange resin to capture smaller particles and soluble impurities; the number of layers of the deep filter material is 3-6; the pore size range of the deep filter material gradually transitions from 1-5 microns to 0.1-1 microns; the flow rate and pressure in the main filtration process are monitored in real time by flow meters and pressure gauges; D4 filtration test: Take samples regularly and use atomic absorption spectroscopy to check the purity of the solution. If the test fails, adjust the filtration speed and pressure through the filtration control system; or replace the precision microporous filter membrane and deep filtration material.

Citation Information

Patent Citations

  • Chemical deep purification method of lithium hexafluorophosphate

    CN103553009A

  • Method for synthesizing lithium hexafluorophosphate solution by using fluorine-containing waste residues

    CN113651341A

  • Preparation method of lithium hexafluorophosphate and lithium ion battery electrolyte containing lithium hexafluorophosphate

    CN114865091A

  • Preparation method of liquid lithium hexafluorophosphate, electrolyte and lithium ion battery

    CN115583661A