Low-density heat-proof material and preparation method thereof

By using base rubber, ablation-resistant fillers, modified hollow fibers, lightweight fillers and other constituent materials, heat-proof materials with low density, high mechanical properties and good thermal insulation properties are prepared, which solves the problem of material properties and problems in the existing technology. The issue of process complexity is applicable to the thermal protection of new generation aircraft.

CN118791876APending Publication Date: 2024-10-18湖北航聚科技股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411077456.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

It is difficult for existing low-density heat-proof materials to maintain good mechanical properties and thermal insulation properties while reducing density. The preparation process is complex and energy consumption is high, which limits their application in aerospace vehicles.

Method used

It adopts low-density heat-proof materials composed of base rubber, ablation-resistant fillers, hollow fibers modified by surface modifiers, lightweight fillers, heat stabilizers and curing agents, and is prepared through mixing, stirring and spray molding processes. Forming a material with high mechanical properties and good thermal insulation properties.

Benefits of technology

It is possible to maintain high mechanical properties and good thermal insulation properties while reducing material density, simplifying the preparation process, improving the payload capacity of the aircraft, and meeting the thermal protection needs of the new generation of aircraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791876A_ABST
    Figure CN118791876A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermal insulation materials, and particularly relates to a low-density thermal insulation material and a preparation method thereof. The low-density heat-proof material is prepared from the following raw materials: base rubber, ablation-resistant filler, hollow fibers modified by a surface modifier, light filler, a heat stabilizer, a curing agent and a solvent. The low-density heat-proof material has the advantages of being high in mechanical property, low in density and good in heat-proof performance, the effective load of an aircraft can be effectively improved, the aircraft can meet the heat protection requirement of a new generation of aircrafts, the preparation method of the low-density heat-proof material is simple, and the low-density heat-proof material has a good application prospect in the field of heat-proof materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat-insulating materials, and in particular relates to a low-density heat-insulating material and a preparation method thereof. Background Art

[0002] Thermal Protection System (TPS) is a structure used to protect spacecraft from burning and overheating in an aerodynamic heating environment. Ablation heat protection has become the main heat protection method for reentry vehicles due to its safety, reliability, strong ability to adapt to external heating changes, and high thermal protection efficiency.

[0003] Since the beginning of the 21st century, along with the gradual development of the country's aerospace industry, ablative heat-resistant materials are facing an urgent need to reduce weight. The lightweighting of heat-resistant materials is a major scientific and engineering technology issue that is constantly emphasized on the premise of meeting the heat protection needs. Studies have shown that for every 1kg reduction in the mass of the spacecraft, the effective range of the strategic missile warhead will increase by more than 20km, and the launch vehicle can save about 50kg of fuel. Therefore, for the future development of deep space exploration, manned lunar landing and new spacecraft, reducing the mass of heat-resistant materials can increase the payload of the aircraft. However, while reducing the density of the heat-resistant material, its mechanical properties, such as tensile strength, elongation at break, and ablation resistance will decrease. Therefore, while reducing the density of the heat-resistant material, it can also ensure that its mechanical properties can meet the use requirements. This is an urgent problem to be solved. At present, there have been many studies on this aspect.

[0004] Patent application CN109266212A proposes a low-density, high-performance heat-resistant coating. The material uses silicone rubber filled with hollow glass balls and fumed silica. It has the characteristics of low density and low thermal conductivity. However, the density of this series of heat-resistant materials is 0.5-0.7g / cm 3 , thermal conductivity ≤0.14W / (m·k). Due to the limitation of hollow microsphere density and the number of added portions, the density and thermal conductivity of the coating material cannot be further reduced, which limits its performance improvement and application areas.

[0005] Patent application CN109294238A proposes a lightweight, highly elastic, ablation-resistant thermal insulation material and its preparation method. The material is composed of heat-vulcanized silicone rubber, boron phenolic resin, hexamethylenetetramine, white carbon black, hydroxy silicone oil, lightweight ablation-resistant filler, vulcanizer, mesitylene and fiber. It is formed by mixing, plasticating, banburying, and multiple staged foaming and vulcanization. It has good elasticity and ablation resistance, but has a high density of 0.6-0.8 / cm 3 The molding process is also relatively complicated, requiring multiple stages of high-temperature foaming (90°C, 150°C, 170°C, 190°C), which has high requirements on equipment and high energy consumption.

[0006] Patent application CN109796772A proposes a flexible ablation-resistant composite material of an air-source micro-foamed carbon layer. The material is composed of silicone rubber, fiber, white carbon black, air-source material, curing agent and catalyst, and is molded at room temperature. It has good ablation resistance, but the thermal conductivity of the material is 0.18-0.29W / (m·k), the thermal insulation performance is poor, and the process is complicated.

[0007] Patent application CN115304918A proposes a low-density solid engine heat protection material and its preparation method. The material is composed of silicone resin, reinforcing filler, fiber, pulp, curing agent and catalyst, etc., and is cured at room temperature. The production process is simple. The prepared material has a "three-phase" structure and has a low density of 0.3-0.4g / cm 3 , has good thermal insulation properties, but it is limited by the fiber swelling capacity and pores, and its ability to reduce the density of the material is limited.

[0008] Patent application CN107459359A proposes a silicon dioxide-based lightweight ceramic thermal protection material, which uses a rigid thermal insulation tile as the base, composite Si-OC aerogel, and is coated with a strengthening coating on the surface. The resulting material has a low density, with a protective material density as low as 0.20-0.25 g / cm 3 , has good thermal insulation performance, and the thermal conductivity is 0.05~0.1W / (m·K), but it requires supercritical drying technology, which has harsh conditions, complex process and high cost. Summary of the invention

[0009] Based on the above technical background, the main purpose of the present invention is to provide a low-density heat-resistant material and a preparation method thereof to overcome the deficiencies in the prior art.

[0010] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0011] The first aspect of the present invention is to provide a low-density heat-proof material, wherein the low-density heat-proof material is made of the following raw materials in parts by weight:

[0012] 800 parts of base rubber, 100-400 parts of ablation-resistant filler, 80-120 parts of hollow fibers modified by a surface modifier, 200-300 parts of lightweight filler, 80-120 parts of heat stabilizer, 8-80 parts of curing agent, and 400-600 parts of solvent.

[0013] Preferably, the low-density heat-proof material is made from the following raw materials in parts by weight:

[0014] 800 parts of base rubber, 300 parts of ablation-resistant filler, 100 parts of hollow fibers modified by a surface modifier, 250 parts of lightweight filler, 100 parts of heat stabilizer, 50 parts of curing agent, and 500 parts of solvent.

[0015] Preferably, the base glue comprises liquid silicone rubber and liquid silicone resin, the silicone rubber is selected from one or more of methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber, and methyl vinyl boron silicon rubber; the silicone resin is selected from one or more of methyl vinyl silicone resin, methyl vinyl phenyl silicone resin, and methyl vinyl boron silicon resin; and / or,

[0016] The ablation-resistant filler is selected from one or more of fumed silica, fumed titania, silicon powder, quartz powder, glass powder, mullite fiber powder, basalt fiber powder, aramid powder, polyimide powder, polyphenylene benzobisoxazole powder, and nano-alumina; and / or,

[0017] The lightweight filler is selected from one or more of hollow glass microspheres, hollow phenolic microspheres, cork powder, silicone microspheres, and aerogel powder; and / or,

[0018] The heat stabilizer is selected from one or more of iron oxide powder, cerium oxide powder, zirconium oxide powder, or zinc oxide powder; and / or,

[0019] The solvent is selected from one or more of n-hexane, cyclohexane, n-heptane, ethyl acetate, butyl acetate and toluene; and / or,

[0020] The curing agent comprises an inhibitor, a cross-linking agent and a catalyst; the mass ratio of the inhibitor, the cross-linking agent and the catalyst is 30-40:2-5:8-15; and / or,

[0021] The hollow fiber modified with a surface modifier is obtained by modifying the hollow fiber with a surface modifier.

[0022] More preferably, the inhibitor is selected from one or more of 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-butyn-3-ol, 2-methyl-3-butyn-2-ol; and / or,

[0023] The cross-linking agent is selected from one or more of methyl hydrogen-containing silicone oil, phenyl hydrogen-containing silicone oil, methyl hydrogen-containing silicone resin, and phenyl hydrogen-containing silicone resin; and / or,

[0024] The catalyst is selected from one or more of platinum-vinyl alkoxysilane complexes and platinum-alkyne complexes.

[0025] More preferably, the surface modifier comprises a silane coupling agent and a titanate coupling agent, the silane coupling agent is KH550, KH560 or KH570, and the titanate coupling agent is TMC-201 or TMC-105; and / or,

[0026] The hollow fiber is selected from one or more of hollow quartz fiber, hollow alumina fiber, hollow carbon nanotube fiber, hollow polytetrafluoroethylene fiber, and hollow polyester fiber.

[0027] More preferably, the mass ratio of the hollow fiber to the surface modifier is 50:0.5-5.

[0028] The second aspect of the present invention is to provide a method for preparing the low-density heat-proof material according to the first aspect of the present invention, the method comprising the following steps:

[0029] Step 1, mixing the base rubber, the ablation-resistant filler and the heat stabilizer to obtain a mixed material;

[0030] Step 2: Add lightweight fillers, hollow fibers modified by a surface modifier, and solvents to the mixed material, stir and disperse, then add a curing agent, spray and form, and cure to obtain a low-density heat-resistant material.

[0031] Preferably, in step 1,

[0032] The base rubber, the ablation-resistant filler and the heat stabilizer are mixed for 10 to 30 minutes to obtain a mixed material.

[0033] Preferably, in step 2,

[0034] Lightweight fillers, hollow fibers modified by surface modifiers and solvents are added to the mixed material, stirred and dispersed at a stirring speed of 400 to 600 r / min for 10 to 30 minutes, and then a curing agent is added for spraying and molding, and then cured at room temperature for 5 to 10 days.

[0035] Preferably, in step 2,

[0036] The hollow fiber modified by the surface modifier is prepared by the following steps:

[0037] The hollow fiber, solvent and surface modifier are mixed, and the temperature is raised to react under argon protection. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed and vacuum dried to obtain the hollow fiber modified by the surface modifier.

[0038] The beneficial effects of the present invention are:

[0039] (1) The low-density heat-proof material of the present invention introduces hollow fibers, and utilizes the characteristics of the hollow fiber tube wall being uneven and having a large number of active sites. After the surface of the hollow fiber and the light filler is modified with a surface modifier, the physical and chemical interactions between the components in the material can be increased, thereby improving the mechanical properties of the low-density heat-proof material;

[0040] (2) The present invention adjusts the usage ratio of hollow fibers to lightweight fillers, utilizes the self-supporting ability and hollow structure of the hollow fibers themselves, and interlaces with the fillers inside the material to form a large number of pore structures similar to "beaver nests", thereby significantly reducing the material density while ensuring that the material has high mechanical properties;

[0041] The gaps formed by the hollow fibers and lightweight fillers inside the material are filled with air, and the low thermal conductivity of air can further improve the thermal insulation performance of the coating. At the same time, the hollow structure of the hollow fibers is conducive to guiding the release of the pyrolysis gas generated inside the coating, solving the problem of bulging and cracking of the coating at high temperatures.

[0042] (3) The preparation method of the low-density heat-resistant material of the present invention is simple, and the prepared material has the advantages of high mechanical properties, low density, and good heat-resistant performance, which can effectively increase the payload of the aircraft and enable it to meet the thermal protection requirements of the new generation of aircraft. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A photograph of the low-density heat-resistant material prepared in Example 1 after ablation is shown. DETAILED DESCRIPTION

[0044] The present invention will be described in detail below, and the characteristics and advantages of the present invention will become clearer and more distinct with the description.

[0045] The first aspect of the present invention is to provide a low-density heat-proof material, wherein the low-density heat-proof material is made of the following raw materials in parts by weight:

[0046] 800 parts of base rubber, 100-400 parts of ablation-resistant filler, 80-120 parts of hollow fibers modified by a surface modifier, 200-300 parts of lightweight filler, 80-120 parts of heat stabilizer, 8-80 parts of curing agent, and 400-600 parts of solvent.

[0047] Preferably, the low-density heat-proof material is made of raw materials including the following parts by weight: 800 parts of base glue, 300 parts of ablation-resistant filler, 100 parts of hollow fibers modified by a surface modifier, 250 parts of lightweight filler, 100 parts of heat stabilizer, 50 parts of curing agent, and 500 parts of solvent.

[0048] The base rubber includes liquid silicone rubber and liquid silicone resin, the silicone rubber is selected from one or more of methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber, and methyl vinyl borosilicate rubber; the silicone resin is selected from one or more of methyl vinyl silicone resin, methyl vinyl phenyl silicone resin, and methyl vinyl borosilicate resin.

[0049] Preferably, the base rubber is methyl vinyl phenyl silicone rubber.

[0050] The ablation-resistant filler is selected from one or more of fumed silica, fumed titanium dioxide, silicon powder, quartz powder, glass powder, mullite fiber powder, basalt fiber powder, aramid powder, polyimide powder, polyphenylene benzobisoxazole powder, and nano-alumina; the size of the ablation-resistant filler is 400-1000 mesh.

[0051] Preferably, the ablation-resistant filler is a mixture of fumed silica and polyimide powder, and the mass ratio of the fumed silica to the polyimide powder is 2:1.

[0052] The light filler is selected from one or more of hollow glass microspheres, hollow phenolic microspheres, cork powder, silicone resin microspheres, and aerogel powder, and the size of the light filler is 400-800 meshes.

[0053] Preferably, the lightweight filler is hollow glass microspheres.

[0054] The heat stabilizer is selected from one or more of iron oxide powder, cerium oxide powder, zirconium oxide powder, or zinc oxide powder; the size of the heat stabilizer is 400-800 meshes.

[0055] Preferably, the thermal stabilizer is iron oxide powder.

[0056] The solvent is selected from one or more of n-hexane, cyclohexane, n-heptane, ethyl acetate, butyl acetate and toluene.

[0057] Preferably, the solvent is ethyl acetate.

[0058] The curing agent comprises an inhibitor, a cross-linking agent and a catalyst; the mass ratio of the inhibitor, the cross-linking agent and the catalyst is 30-40:2-5:8-15.

[0059] The inhibitor is selected from one or more of 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-butyn-3-ol, and 2-methyl-3-butyn-2-ol; preferably 1-ethynylcyclohexanol.

[0060] The crosslinking agent is selected from one or more of methyl hydrogen-containing silicone oil, phenyl hydrogen-containing silicone oil, methyl hydrogen-containing silicone resin, and phenyl hydrogen-containing silicone resin; preferably, phenyl hydrogen-containing silicone oil.

[0061] The catalyst is selected from one or more of platinum-vinyl alkoxy silane complexes and platinum-alkyne complexes, preferably platinum-vinyl alkoxy silane complexes.

[0062] The surface modifier is one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a zirconate aluminate coupling agent or stearic acid.

[0063] The hollow fiber modified by the surface modifier is obtained by modifying the hollow fiber by the surface modifier, the surface modifier comprises a silane coupling agent and a titanate coupling agent, the silane coupling agent is KH550, KH560 or KH570, and the titanate coupling agent is TMC-201 or TMC-105.

[0064] Preferably, the surface modifier is one or both of KH560 and TMC-201.

[0065] The hollow fiber is selected from one or more of hollow quartz fiber, hollow alumina fiber, hollow carbon nanotube fiber, hollow polytetrafluoroethylene fiber, and hollow polyester fiber; the diameter of the hollow fiber is 1 to 100 μm, and the aspect ratio is (1 to 30):1.

[0066] Preferably, the hollow fiber is selected from one or both of hollow quartz fiber and hollow carbon nanotube fiber.

[0067] More preferably, the hollow fiber is obtained by mixing hollow quartz fiber and hollow carbon nanotube fiber in a mass ratio of 1:1.

[0068] The mass ratio of the hollow fiber to the surface modifier is 50:0.5-5, and the preferred mass ratio is 50:1.5.

[0069] The second aspect of the present invention is to provide a method for preparing the low-density heat-proof material according to the first aspect of the present invention, the method comprising the following steps:

[0070] Step 1, mixing the base rubber, the ablation-resistant filler and the heat stabilizer to obtain a mixed material;

[0071] Step 2: Add lightweight fillers, hollow fibers modified by a surface modifier, and solvents to the mixed material, stir and disperse, then add a curing agent, spray and form, and cure to obtain a low-density heat-resistant material.

[0072] The above steps are described in detail below.

[0073] In step 1, the mixing is preferably carried out in an open mixer, and the base rubber, ablation-resistant filler, and heat stabilizer are mixed for 10 to 30 minutes to obtain a mixed material, preferably for 20 minutes to obtain a mixed material.

[0074] In step 2, stirring and dispersing is preferably carried out in a disperser, and a lightweight filler, a hollow fiber modified by a surface modifier and a solvent are added to the mixed material, and stirred and dispersed at a stirring speed of 400 to 600 r / min for 10 to 30 minutes, and then a curing agent is added for spraying and molding, and then cured at room temperature for 5 to 10 days.

[0075] Preferably, light fillers, hollow fibers modified by a surface modifier and solvents are added to the mixed material, stirred and dispersed at a stirring speed of 500 r / min for 20 minutes, and then a curing agent is added for spraying and molding, and then cured at room temperature for 7 days to obtain the product.

[0076] The hollow fiber modified by the surface modifier is prepared by the following steps:

[0077] The hollow fiber, solvent and surface modifier are mixed, and the temperature is raised to react under argon protection. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed and vacuum dried to obtain the hollow fiber modified by the surface modifier.

[0078] Preferably, the hollow fiber, toluene and the surface modifier are mixed, and the temperature is raised to 80-100° C. and kept for reaction for 2-4 hours under argon protection. After the reaction is completed, the mixture is cooled to room temperature, the toluene is removed by suction filtration, and the mixture is washed twice with acetone and vacuum dried at 60-80° C. for 1-3 hours to obtain the hollow fiber modified with the surface modifier.

[0079] More preferably, the hollow fiber, toluene and surface modifier are mixed, and the temperature is raised to 90°C for reaction for 3 hours under argon protection. After the reaction is completed, it is cooled to room temperature, the toluene is removed by suction, and the mixture is washed twice with acetone and vacuum dried at 70°C for 2 hours to obtain a hollow fiber modified with a surface modifier.

[0080] Example

[0081] The present invention is further described below by specific examples, which are limited to illustrating the present invention but not to limiting the scope of the present invention. The raw materials used in the examples of the present invention were all purchased.

[0082] Example 1

[0083] (1) Surface modification of hollow fibers: 500 g of hollow quartz fiber with a diameter of 10 μm and an aspect ratio of 20:1 was placed in a three-necked flask, 2000 g of toluene and 15 g of KH560 were added, magnetic stirring was performed and argon was introduced, the temperature was raised to 90°C, and the reaction was kept warm for 3 h. After the reaction was completed, the fiber was cooled to room temperature, the toluene was removed by filtration, and the fiber was washed twice with acetone and placed in a vacuum drying oven and dried at 70°C for 2 h to obtain the modified hollow quartz fiber.

[0084] (2) Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica (size of 400-1000 mesh), 100g of polyimide powder (size of 400-1000 mesh), and 100g of iron oxide powder (400-800 mesh), place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres (size of 400-800 mesh), 100g of modified hollow quartz fiber, and 500g of ethyl acetate to the mixed material, and use a disperser to stir and disperse at 500r / min for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0085] Example 2

[0086] (1) Surface modification of hollow carbon nanotubes: 500 g of hollow carbon nanotubes with a diameter of 50 nm and an aspect ratio of 20:1 were placed in a three-necked flask, 2000 g of toluene and 15 g of TMC-201 were added, magnetic stirring was performed and argon gas was introduced, the temperature was raised to 90°C, and the reaction was kept warm for 3 h. After the reaction was completed, the mixture was cooled to room temperature, the toluene was removed by filtration, and the mixture was washed twice with acetone and placed in a vacuum drying oven and vacuum dried at 70°C for 2 h to obtain the modified hollow carbon nanotubes.

[0087] (2) Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica (size of 400-1000 mesh), 100g of polyimide powder (size of 400-1000 mesh), and 100g of iron oxide powder (400-800 mesh), place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres (size of 400-800 mesh), 100g of modified hollow carbon nanotubes, and 500g of ethyl acetate to the mixed material, and use a disperser to stir and disperse at 500r / min for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0088] Example 3

[0089] (1) Surface modification of hollow fibers: 500 g of hollow quartz fiber with a diameter of 10 μm and an aspect ratio of 20:1 was placed in a three-necked flask, 2000 g of toluene and 15 g of KH560 were added, magnetic stirring was performed and argon was introduced, the temperature was raised to 90°C, and the reaction was kept warm for 3 h. After the reaction was completed, the fiber was cooled to room temperature, the toluene was removed by filtration, and the fiber was washed twice with acetone and placed in a vacuum drying oven and dried at 70°C for 2 h to obtain the modified hollow quartz fiber.

[0090] (2) Surface modification of hollow carbon nanotubes: 500 g of hollow carbon nanotubes with a diameter of 50 nm and an aspect ratio of 20:1 were placed in a three-necked flask, 2000 g of toluene and 15 g of TMC-201 were added, magnetic stirring was performed and argon gas was introduced, the temperature was raised to 90°C, and the reaction was kept warm for 3 h. After the reaction was completed, the flask was cooled to room temperature, the toluene was removed by filtration, and the flask was washed twice with acetone and placed in a vacuum drying oven and vacuum dried at 70°C for 2 h to obtain the modified hollow carbon nanotubes.

[0091] (3) Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica (size of 400-1000 mesh), 100g of polyimide powder (size of 400-1000 mesh), and 100g of iron oxide powder (400-800 mesh), place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres (size of 400-800 mesh), 50g of modified hollow quartz fiber, 50g of modified hollow carbon nanotubes, and 500g of ethyl acetate to the mixed material, and use a disperser to stir and disperse at 500r / min for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0092] Comparative Example

[0093] Comparative Example 1

[0094] A method for preparing a low-density heat-resistant material comprises the following steps:

[0095] Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica, 100g of polyimide powder, and 100g of iron oxide, place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres, 100g of hollow quartz fiber with a diameter of 10μm and an aspect ratio of 20:1, and 500g of ethyl acetate to the mixed material, and use a disperser to stir and disperse for 20 minutes at 500r / min. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0096] Comparative Example 2

[0097] A method for preparing a low-density heat-resistant material comprises the following steps:

[0098] Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica, 100g of polyimide powder, and 100g of iron oxide, place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres, 100g of solid quartz fiber with a diameter of 10μm and an aspect ratio of 20:1, and 500g of ethyl acetate to the mixed material, and use a disperser at 500r / min to stir and disperse for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0099] Comparative Example 3

[0100] A method for preparing a low-density heat-resistant material comprises the following steps:

[0101] Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica, 100g of polyimide powder, and 100g of iron oxide, place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 250g of hollow glass microspheres and 500g of ethyl acetate to the mixed material, and use a disperser at 500r / min to stir and disperse for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol, and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0102] Comparative Example 4

[0103] A method for preparing a low-density heat-resistant material comprises the following steps:

[0104] Weigh 800g of methyl vinyl phenyl silicone rubber, 200g of fumed silica, 100g of polyimide powder, and 100g of iron oxide, place them on an open mill and mix them for 20 minutes to obtain a mixed material. Add 400g of hollow glass microspheres and 700g of ethyl acetate to the mixed material, and use a disperser at 500r / min to stir and disperse for 20 minutes. Add 40g of phenyl hydrogenated silicone oil, 2g of 1-ethynyl cyclohexanol and 8g of platinum-vinyl alkoxysilane complex, stir evenly, and then use a spraying process to form. After curing at room temperature for 7 days, a low-density heat-resistant material is obtained.

[0105] Experimental example

[0106] Experimental Example 1 Performance Test

[0107] The low-density heat-resistant materials prepared in Examples 1-3 and Comparative Examples 1-4 were tested for mechanical properties, density, thermal conductivity and ablation performance. The test standards and test results are shown in Table 1. The photo of Example 1 after ablation is shown in Table 1. Figure 1 shown.

[0108] Table 1 Performance test results

[0109]

[0110]

[0111] As can be seen from Table 1, in Comparative Example 1, the hollow fibers are not subjected to surface treatment. Compared with Examples 1-3, the interaction force of the components of the obtained material is poor, and the density, tensile strength, elongation at break and other properties of the material obtained in Comparative Example 1 are all reduced.

[0112] Comparative Example 2 does not add hollow fibers. From the performance test results, its density is 0.35 g / cm 3 , it cannot effectively reduce the density of the material, and at the same time, it shows local overburning phenomenon.

[0113] Comparative Example 3 does not add fiber fillers. From the performance test results, the heat-resistant material obtained has a high density and poor ablation resistance.

[0114] Comparative Example 4: Increasing the amount of glass hollow microspheres added, the performance test results show that the density of the heat-resistant material can be reduced to 0.30 g / cm 3 However, its tensile strength and elongation at break are too low, and its ablation performance is poor, which cannot meet the practical application requirements.

[0115] It can be seen from the comparison of Examples 1-3 that the use of hollow carbon nanotubes instead of hollow quartz fibers in Example 2 can reduce the density of the material and improve the material's ablation resistance; the use of modified hollow quartz fibers in combination with carbon nanotube fibers in Example 3 can reduce the density of the heat-resistant material while ensuring that it has good mechanical properties and ablation resistance and thermal insulation properties. Figure 1 It can be seen that the low-density heat-resistant material prepared in Example 1 has good ablation resistance.

[0116] The above results show that the low-density heat-proof material of the present invention has an extremely low density (0.22 g / cm 3 About), good ablation resistance and thermal conductivity.

[0117] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A low-density heat-proof material, characterized in that: The low-density heat-proof material is made from the following raw materials in parts by weight: 800 parts of base rubber, 100-400 parts of ablation-resistant filler, 80-120 parts of hollow fibers modified by a surface modifier, 200-300 parts of lightweight filler, 80-120 parts of heat stabilizer, 8-80 parts of curing agent, and 400-600 parts of solvent.

2. The low-density heat-proof material according to claim 1, characterized in that: The low-density heat-proof material is made from the following raw materials in parts by weight: 800 parts of base rubber, 300 parts of ablation-resistant filler, 100 parts of hollow fibers modified by a surface modifier, 250 parts of lightweight filler, 100 parts of heat stabilizer, 50 parts of curing agent, and 500 parts of solvent.

3. The low-density heat-proof material according to claim 1, characterized in that: The base rubber comprises liquid silicone rubber and liquid silicone resin, wherein the silicone rubber is selected from one or more of methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber, and methyl vinyl borosilicate rubber; the silicone resin is selected from one or more of methyl vinyl silicone resin, methyl vinyl phenyl silicone resin, and methyl vinyl borosilicate resin; and / or, The ablation-resistant filler is selected from one or more of fumed silica, fumed titania, silicon powder, quartz powder, glass powder, mullite fiber powder, basalt fiber powder, aramid powder, polyimide powder, polyphenylene benzobisoxazole powder, and nano-alumina; and / or, The lightweight filler is selected from one or more of hollow glass microspheres, hollow phenolic microspheres, cork powder, silicone microspheres, and aerogel powder; and / or, The heat stabilizer is selected from one or more of iron oxide powder, cerium oxide powder, zirconium oxide powder, or zinc oxide powder; and / or, The solvent is selected from one or more of n-hexane, cyclohexane, n-heptane, ethyl acetate, butyl acetate and toluene; and / or, The curing agent comprises an inhibitor, a cross-linking agent and a catalyst; the mass ratio of the inhibitor, the cross-linking agent and the catalyst is 30-40:2-5:8-15; and / or, The hollow fiber modified with a surface modifier is obtained by modifying the hollow fiber with a surface modifier.

4. The low-density heat-proof material according to claim 3, characterized in that: The inhibitor is selected from one or more of 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-butyn-3-ol, and 2-methyl-3-butyn-2-ol; and / or, The cross-linking agent is selected from one or more of methyl hydrogen-containing silicone oil, phenyl hydrogen-containing silicone oil, methyl hydrogen-containing silicone resin, and phenyl hydrogen-containing silicone resin; and / or, The catalyst is selected from one or more of platinum-vinyl alkoxysilane complexes and platinum-alkyne complexes.

5. The low-density heat-proof material according to claim 3, characterized in that: The surface modifier comprises a silane coupling agent and a titanate coupling agent, wherein the silane coupling agent is KH550, KH560 or KH570, and the titanate coupling agent is TMC-201 or TMC-105; and / or, The hollow fiber is selected from one or more of hollow quartz fiber, hollow alumina fiber, hollow carbon nanotube fiber, hollow polytetrafluoroethylene fiber, and hollow polyester fiber.

6. The low-density heat-proof material according to claim 3, characterized in that: The mass ratio of the hollow fiber to the surface modifier is 50:0.5-5.

7. A method for preparing the low-density heat-protection material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: Step 1, mixing the base rubber, the ablation-resistant filler and the heat stabilizer to obtain a mixed material; Step 2: Add lightweight fillers, hollow fibers modified by a surface modifier, and solvents to the mixed material, stir and disperse, then add a curing agent, spray and form, and cure to obtain a low-density heat-resistant material.

8. The method according to claim 7, characterized in that In step 1, The base rubber, the ablation-resistant filler and the heat stabilizer are mixed for 10 to 30 minutes to obtain a mixed material.

9. The method according to claim 7, characterized in that: In step 2, Lightweight fillers, hollow fibers modified by surface modifiers and solvents are added to the mixed material, stirred and dispersed at a stirring speed of 400 to 600 r / min for 10 to 30 minutes, and then a curing agent is added for spraying and molding, and then cured at room temperature for 5 to 10 days.

10. The method according to claim 7, characterized in that In step 2, The hollow fiber modified by the surface modifier is prepared by the following steps: The hollow fiber, solvent and surface modifier are mixed, and the temperature is raised to react under argon protection. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed and vacuum dried to obtain the hollow fiber modified by the surface modifier.

Citation Information

Cited By

  • 3D printing rubber thermal insulation material and preparation method thereof

    CN121136455A