Swelling adhesive tape for lithium battery and preparation method of swelling adhesive tape
By adopting a three-layer structure of swelling tape for lithium batteries, combined with specific material formulas and hierarchical design, the existing technology's problems of poor resistance and low expansion rate of swelling tapes for lithium batteries in high temperatures and electrolytes are solved, achieving high efficiency. Filling the gap between the battery core and the casing improves the safety and stability of the battery.
Patent Information
- Application Number
- CN202411043180.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
AI Technical Summary
Existing swelling tapes for lithium batteries have poor resistance to high temperatures and electrolytes, low expansion rates, and short service life. They cannot effectively fill the gap between the battery core and the casing, affecting battery performance and safety.
The swelling tape for lithium batteries adopts a three-layer structure, including a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating. It is made of specially formulated polyurethane resin, polyacrylic resin, amino resin curing agent and isocyanate curing agent. Mixed to form a coating with high temperature resistance, electrolyte resistance and high expansion rate, ensuring strength and shape retention in three dimensions.
It can maintain a high expansion ratio at high temperatures without shrinking, and can be soaked in electrolyte for a long time without deformation or dissolution, extending the service life, improving the wear resistance and adhesion of the tape, effectively filling the gap between the battery core and the case, and improving the performance of the tape. Battery safety and stability.
Smart Images

Figure CN118791985A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of swelling tapes, and in particular to a swelling tape for lithium batteries and a preparation method thereof. Background Art
[0002] Expansion tape is a kind of tape with synthetic rubber or resin as the base material, which has excellent oil surface adhesion, operability, expansion, filling, elasticity and good adhesion. With the continuous development of the new energy industry, lithium-ion batteries have received extensive attention due to their own excellent performance. In the manufacturing process of lithium-ion batteries, some gaps are often reserved between the battery cells and the object, but the existence of the gap will cause the mutual movement between the battery cells and the shell, causing the battery to short-circuit and enlarge the battery, which greatly increases the safety hazards during the use of the battery. In order to solve the above problems, the industry mainly uses expansion winding on the battery cell for fixing, but the expansion tapes on the market often have poor high temperature resistance, low expansion rate, no molding after long-term immersion in the electrolyte, low viscosity, short service life and other problems.
[0003] At present, the base materials used in the swelling tape for lithium batteries mostly swell in the thickness direction, and the swelling ratio in the thickness direction is limited, which cannot effectively fill the gap between the bare lithium battery cell and the cylindrical shell. In addition, during the long-term use of the battery, the tape is easy to debond after being exposed to high temperature and soaked in electrolyte. After swelling, the mechanics of the base layer decreases and it dissolves out of shape, affecting the performance of the battery.
[0004] Therefore, a swelling tape with simple process, strong high temperature resistance, high electrolyte resistance and high swelling ratio is provided, which can expand at a high ratio in the electrolyte and maintain a certain strength and shape in three-dimensional directions, and can effectively fill the gap between the bare lithium battery cell and the cylindrical shell, and has great research significance and application prospects. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present application provides a swelling tape for lithium batteries and a preparation method thereof. The swelling tape for lithium batteries of the present application has a simple preparation process, strong high temperature resistance, high electrolyte resistance, and high rate of expansion by absorbing electrolyte, and can maintain a certain strength and shape in three-dimensional directions, and does not shrink at high temperatures. It is applied to new energy lithium batteries and cylindrical lithium batteries to fill the gap between the battery cell and the shell, solving the problems of poor high temperature resistance, low expansion rate, no molding after long-term immersion in electrolyte, low viscosity, and short service life of the existing swelling tape.
[0006] In a first aspect, the present application provides a swelling tape for a lithium battery, which adopts the following technical solution: A swelling tape for lithium batteries, the swelling tape comprising, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, the release agent coating having a thickness of 0.5-1 μm, the polyurethane swelling coating having a thickness of 10-50 μm, and the electrolyte-resistant acrylic coating having a thickness of 2-10 μm, wherein the electrolyte-resistant acrylic coating is prepared from raw materials comprising, by weight, 50-100 parts of a polyurethane resin, 5-30 parts of a polyacrylic resin, 0.5-5 parts of an amino resin curing agent, 0.5-10 parts of an isocyanate curing agent, and 55-140 parts of a solvent.
[0007] By adopting the above technical scheme, the swelling tape for lithium batteries of the present application is composed of three layers, each of which has its unique role and function, and there is also a synergistic effect between them. Release agent coating: The main function of this layer is to prevent the tape from sticking during storage or use, and to ensure that the tape can be smoothly unfolded and used. The thickness of the release agent coating is controlled between 0.5-1μm, which is sufficient to provide the necessary anti-sticking effect without adversely affecting the overall performance. Polyurethane swelling coating: Responsible for absorbing electrolyte and swelling. Its thickness is between 10-50μm, and can be adjusted according to actual needs to control the degree of expansion. The design of the polyurethane swelling coating enables it to expand rapidly in the electrolyte, fill the gap between the battery cell and the shell, thereby improving the safety and stability of the battery. Electrolyte-resistant acrylic coating: This layer is located on the outermost layer and is in direct contact with the electrolyte. Its main function is to protect the internal polyurethane swelling coating from electrolyte erosion, while improving the temperature resistance and chemical resistance of the entire tape. The thickness of the electrolyte-resistant acrylic coating is 2-10 μm, and excellent protective performance is achieved by mixing a specific formula of polyurethane resin, polyacrylic resin, curing agent and solvent. In the swelling tape for lithium batteries of the present application, the role and synergistic effect of each component in its electrolyte-resistant acrylic coating are as follows: Polyurethane resin: As the main film-forming material, it provides good adhesion and flexibility, and has good electrolyte resistance. It can remain stable at high temperatures and is not prone to shrinkage and deformation. Polyacrylic resin: When used in combination with polyurethane resin, the electrolyte resistance and high temperature resistance of the coating are improved. At the same time, polyacrylic resin has good adhesion, which helps to improve the adhesion between the coating and the substrate. Amino resin curing agent: As a cross-linking agent, it reacts with polyurethane resin and polyacrylic resin to form a three-dimensional network structure, which improves the electrolyte resistance and high temperature resistance of the coating. At the same time, the amino resin curing agent can also improve the hardness and wear resistance of the coating. Isocyanate curing agent: As another cross-linking agent, it reacts with polyurethane resin and polyacrylic resin to form a three-dimensional network structure, thereby improving the coating's electrolyte resistance and high temperature resistance. Isocyanate curing agent can also improve the hardness and wear resistance of the coating. Solvent: Used to adjust the viscosity and leveling of the coating to facilitate coating and construction. At the same time, the solvent can also affect the drying speed and curing time of the coating. In summary, the swelling tape for lithium batteries of the present application achieves the goals of high temperature resistance, electrolyte resistance, high expansion rate and long-term stability through its unique three-layer structure and material selection, providing a high-performance solution for new energy lithium batteries and cylindrical lithium batteries.
[0008] Preferably, the polyurethane resin is prepared by mixing thermoplastic polyurethane resin and polyurea polyurethane resin in a mass ratio of 7:1.
[0009] By adopting the above technical scheme, firstly, the thermoplastic polyurethane resin has good temperature resistance, oil resistance and aging resistance, which can effectively improve the high temperature resistance of the swelling tape, so that it can maintain a high expansion ratio at high temperature without shrinking. At the same time, the thermoplastic polyurethane resin also has good elasticity and toughness, which can enhance the strength and toughness of the swelling tape. Secondly, the polyurea polyurethane resin has excellent chemical corrosion resistance and wear resistance, which can improve the electrolyte resistance of the swelling tape, so that it will not deform or dissolve when immersed in the electrolyte for a long time. Finally, by compounding the thermoplastic polyurethane resin and the polyurea polyurethane resin, the synergistic effect of the two can be achieved, and the performance of the swelling tape can be further improved. On the one hand, this compounding can improve the electrolyte resistance and high temperature resistance of the swelling tape, form a three-dimensional structure with a certain strength, and effectively fill the gap between the battery cell and the shell; on the other hand, this compounding can also make the swelling tape have excellent mechanical properties, and can maintain a high expansion ratio at high temperature without shrinking.
[0010] Preferably, the isocyanate curing agent is at least one of toluene diisocyanate and diphenylmethane diisocyanate.
[0011] Preferably, the solvent, by mass, comprises: 50-110 parts of ethyl acetate and 5-30 parts of N,N-dimethylformamide.
[0012] Preferably, the raw materials for preparing the electrolyte-resistant acrylic coating further include, by weight, 5-6 parts of modified silicon dioxide.
[0013] Preferably, the method for preparing the modified silicon dioxide comprises the following steps: S61. Dissolve 8 parts of succinic anhydride in 40-50 parts of N,N-dimethylformamide solution according to mass fractions, add 18 parts of γ-aminopropyltriethoxysilane, heat and stir at a water bath temperature of 73° C. for 2-3 hours to obtain a mixed solution A; S62, dissolving 20 parts by mass of silicon dioxide having an average particle size of 20 nm in 50 parts by mass of N,N-dimethylformamide solution to obtain a mixed solution B; S63, adding the mixed solution B dropwise into the mixed solution A, and continuing to stir and react for 3 hours to obtain pretreated silica; S64, the pretreated silica was mixed with 10 parts of 2-methylimidazole and 8 parts of zinc nitrate hexahydrate, and 140 parts of ethanol were added, and ultrasonic polymerization was performed in an 800 W water bath ultrasonic device for 3-4 hours. The obtained product was washed and dried to obtain modified silica.
[0014] By adopting the above technical scheme, the modified silica prepared increases the adhesion between the electrolyte-resistant acrylic coating and the polyurethane swelling coating, prolongs the service life of the swelling tape, and ensures that no residual glue will remain when the swelling tape is removed. The inventor speculates that: the surface of the unmodified silica still has hydroxyl groups, which is easy to absorb moisture in the air. When applied to organic materials, phase separation often occurs. The surface of the modified silica forms an organic coating layer, which can effectively reduce the surface energy of silica, improve the surface properties of silica, and increase the affinity of silica with organic materials. The strength, toughness, high temperature resistance and electrolyte resistance of the swelling tape are enhanced. The present application further compounds polyurethane resin, polyacrylic resin and modified silica to improve the adsorption performance of the tape, solving the technical problem that the existing expansion glue has poor temperature resistance and poor expansion effect in high-temperature electrolyte. The inventors speculate that the use of a compound of polyurethane resin, polyacrylic resin and modified silica can effectively improve the thermal stability of the electrolyte-resistant acrylic coating, and by improving the temperature resistance of the film, essentially avoid battery accidents caused by the shrinkage and expansion of the swelling tape due to high temperature in the prior art.
[0015] In a second aspect, the present application provides a method for preparing a swelling tape for a lithium battery, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the swelling tape for a lithium battery, comprising the following steps: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating to control the corona value of the polyurethane swelling coating to be ≥56 dynes; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their weight fractions, and after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, respectively adding the amino resin curing agent and the isocyanate curing agent, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying. Then, laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared.
[0016] Preferably, in steps S72 and S74, coating is carried out at a speed of 7-25 m / min, and then entering the oven for drying at the same speed, and the temperatures of oven sections 1-8 are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
[0017] Preferably, in step S73, the polyurethane resin and the polyacrylic resin are dissolved in a solvent according to their mass fractions. After the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, modified silica is added and stirred evenly. Finally, the amino resin curing agent and the isocyanate curing agent are respectively added and stirred evenly to obtain electrolyte-resistant acrylic glue.
[0018] In summary, the present application includes at least one of the following beneficial technical effects: 1. By using modified silica, the adhesion between the electrolyte-resistant acrylic coating and the polyurethane swelling coating is increased, the service life of the swelling tape is extended, and it is ensured that no adhesive residue will remain when the swelling tape is removed.
[0019] 2. By compounding polyurethane resin, polyacrylic resin and modified silica, the adsorption performance of the tape is improved, solving the technical problem that the existing expansion adhesive has poor expansion effect in high-temperature electrolyte due to poor temperature resistance.
[0020] 3. By adding a small amount of polyurea polyurethane resin to the thermoplastic polyurethane resin, the obtained base film electrolyte-resistant acrylic coating swells in an area larger during immersion in the lithium battery electrolyte, forming a three-dimensional structure with a certain strength, effectively filling the gap between the battery cell and the shell.
[0021] 4. The swelling tape has excellent high temperature resistance, can maintain a high expansion ratio at high temperature without shrinking, and will not deform or dissolve when immersed in electrolyte for a long time.
[0022] 5. Through the compounding of polyurethane resin and polyacrylic resin, the electrolyte resistance and high temperature resistance of the swelling tape are significantly improved, forming a three-dimensional structure with a certain strength, which effectively fills the gap between the battery cell and the shell. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following is a brief introduction to the drawings used in the embodiments: Figure 1 This is a schematic diagram of the structure of the swelling tape for lithium batteries prepared in Example 6 of the present application; In the figure, 1 represents a release agent coating; 2 represents a polyurethane swelling coating; 3 represents an electrolyte-resistant acrylic coating; Figure 2This is a product picture of the swelling tape for lithium batteries prepared in Example 6 of the present application. DETAILED DESCRIPTION
[0024] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0025] Preparation Example 1 Preparation of modified silicon dioxide The preparation method of modified silicon dioxide comprises the following steps: S61. Dissolve 80 g of succinic anhydride in 450 g of N,N-dimethylformamide solution according to mass fractions, add 180 g of γ-aminopropyltriethoxysilane, and heat and stir at a water bath temperature of 73° C. for 2.5 hours to obtain a mixed solution A. S62, dissolving 200 g of silicon dioxide having an average particle size of 20 nm in 500 g of N,N-dimethylformamide solution according to mass fractions to obtain a mixed solution B; S63, adding the mixed solution B dropwise into the mixed solution A, and continuing to stir and react for 3 hours to obtain pretreated silica; S64, the pretreated silica was mixed with 100 g of 2-methylimidazole and 80 g of zinc nitrate hexahydrate, and 1400 g of ethanol was added, and ultrasonic polymerization was performed in an 800 W water bath ultrasonic device for 3.5 hours. The obtained product was washed and dried to obtain modified silica.
[0026] Example 1 A swelling tape for lithium batteries, the swelling tape comprising, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, the release agent coating having a thickness of 0.5 μm, the polyurethane swelling coating having a thickness of 50 μm, and the electrolyte-resistant acrylic coating having a thickness of 5 μm, wherein the electrolyte-resistant acrylic coating, by weight, is prepared from raw materials comprising: 50 kg of polyurethane resin, 5 kg of polyacrylic resin, 0.5 kg of amino resin curing agent, 2 kg of toluene diisocyanate, and 55 kg of solvent, the polyurethane resin being prepared by mixing thermoplastic polyurethane resin and polyurea polyurethane resin in a weight ratio of 7:1, and the solvent, by weight, comprising: 50 kg of ethyl acetate and 5 kg of N,N-dimethylformamide.
[0027] The method for preparing the swelling tape for lithium battery comprises the following steps: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating, wherein the corona value of the polyurethane swelling coating after treatment is 56 dynes; coating is performed at a speed of 25 m / min, and then entering into an oven for drying at the same speed, wherein the temperatures of sections 1-8 of the oven are 40° C., 70° C., 90° C., 110° C., 130° C., 130° C., 140° C., and 110° C., respectively; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their weight fractions, and after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, respectively adding an amino resin curing agent and toluene diisocyanate, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying, and then laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared; the coating is carried out at a speed of 25m / min, and then the tape is put into an oven for drying at the same speed. The temperatures of sections 1 to 8 of the oven are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
[0028] Example 2 A swelling tape for lithium batteries, the swelling tape comprising, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, the release agent coating having a thickness of 1 μm, the polyurethane swelling coating having a thickness of 10 μm, and the electrolyte-resistant acrylic coating having a thickness of 10 μm, wherein the electrolyte-resistant acrylic coating, by weight, is prepared from raw materials comprising: 100 kg of polyurethane resin, 30 kg of polyacrylic resin, 5 kg of amino resin curing agent, 10 kg of diphenylmethane diisocyanate, and 140 kg of solvent, the polyurethane resin being prepared by mixing thermoplastic polyurethane resin and polyurea polyurethane resin in a weight ratio of 7:1, and the solvent, by weight, comprising: 110 kg of ethyl acetate and 30 kg of N,N-dimethylformamide.
[0029] The method for preparing the swelling tape for lithium battery comprises the following steps: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating, wherein the corona value of the polyurethane swelling coating after treatment is 60 dynes; coating is performed at a speed of 7 m / min, and then entering into an oven for drying at the same speed, wherein the temperatures of sections 1-8 of the oven are 40° C., 70° C., 90° C., 110° C., 130° C., 130° C., 140° C., and 110° C., respectively; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their weight fractions, and after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, respectively adding an amino resin curing agent and diphenylmethane diisocyanate, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying, and then laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared; the coating is carried out at a speed of 7m / min, and then the tape is put into an oven for drying at the same speed. The temperatures of sections 1 to 8 of the oven are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
[0030] Example 3 A swelling tape for lithium batteries, the swelling tape comprising, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, the release agent coating having a thickness of 0.8 μm, the polyurethane swelling coating having a thickness of 30 μm, and the electrolyte-resistant acrylic coating having a thickness of 7 μm, wherein the electrolyte-resistant acrylic coating, by weight, is prepared from raw materials comprising: 80 kg of polyurethane resin, 15 kg of polyacrylic resin, 3 kg of amino resin curing agent, 7 kg of toluene diisocyanate, and 110 kg of solvent, the polyurethane resin being prepared by mixing thermoplastic polyurethane resin and polyurea polyurethane resin in a weight ratio of 7:1, and the solvent, by weight, comprising: 90 kg of ethyl acetate and 20 kg of N,N-dimethylformamide.
[0031] The method for preparing the swelling tape for lithium battery comprises the following steps: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating, wherein the corona value of the polyurethane swelling coating after treatment is 58 dynes; coating is performed at a speed of 14 m / min, and then entering into an oven for drying at the same speed, wherein the temperatures of sections 1-8 of the oven are 40° C., 70° C., 90° C., 110° C., 130° C., 130° C., 140° C., and 110° C., respectively; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their weight fractions, and after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, respectively adding an amino resin curing agent and toluene diisocyanate, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying, and then laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared; the coating is carried out at a speed of 14m / min, and then the tape is put into an oven for drying at the same speed. The temperatures of sections 1 to 8 of the oven are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
[0032] Example 4 A swelling tape for lithium batteries, the swelling tape comprising, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, the release agent coating having a thickness of 0.8 μm, the polyurethane swelling coating having a thickness of 30 μm, and the electrolyte-resistant acrylic coating having a thickness of 7 μm, wherein the electrolyte-resistant acrylic coating, in terms of mass fractions, is prepared from raw materials comprising: 80 kg of polyurethane resin, 15 kg of polyacrylic resin, 3 kg of amino resin curing agent, 7 kg of toluene diisocyanate, 110 kg of solvent, and 5 kg of modified silicon dioxide, the polyurethane resin being prepared by mixing thermoplastic polyurethane resin and polyurea polyurethane resin in a mass fraction ratio of 7:1, and the solvent, in terms of mass fractions, comprising: 90 kg of ethyl acetate and 20 kg of N,N-dimethylformamide.
[0033] Preferably, the raw materials for preparing the electrolyte resistant acrylic coating, by weight, also include: The method for preparing the swelling tape for lithium battery comprises the following steps: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating, wherein the corona value of the polyurethane swelling coating after treatment is 58 dynes; coating is performed at a speed of 14 m / min, and then entering into an oven for drying at the same speed, wherein the temperatures of sections 1-8 of the oven are 40° C., 70° C., 90° C., 110° C., 130° C., 130° C., 140° C., and 110° C., respectively; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to the mass fractions, adding the modified silica after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, stirring evenly, and finally adding the amino resin curing agent and toluene diisocyanate respectively, stirring evenly, to obtain electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying, and then laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared; the coating is carried out at a speed of 14m / min, and then the tape is put into an oven for drying at the same speed. The temperatures of sections 1 to 8 of the oven are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
[0034] Example 5 The same as Example 4, except that the amount of modified silica added is 6 kg.
[0035] Example 6 The same as Example 4, except that the amount of modified silicon dioxide added is 5.5 kg.
[0036] Comparative Example 1 The same as Example 3, except that: the polyurethane resin is a thermoplastic polyurethane resin.
[0037] Comparative Example 2 The same as Example 3, except that the polyurethane resin is a polyurea polyurethane resin.
[0038] Comparative Example 3 The same as Example 6, except that an equal amount of silicon dioxide is used instead of modified silicon dioxide.
[0039] Performance testing The swelling tapes for lithium batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were sampled and subjected to the following performance tests. The test results are shown in Table 1. Tensile strength and elongation at break test: According to the "Test method for tensile strength and elongation at break of GB / T 30776-2014", the swelling tape for lithium batteries is cut longitudinally to a width of 25mm and a length of not less than 200mm. The distance between the middle specimens of the tensile machine is 100mm, and the specimens are clamped in the upper and lower fixtures. The center line of the fixture is vertical and consistent with the direction of the applied load, and the test machine is started at (5±0.2)mm / s. The results of 5 fracture specimens under normal conditions are obtained; Swelling and shape retention test of swelling tape: The swelling tapes for lithium batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were cut into samples with a length of 55 mm and a width of 58 mm, respectively, and immersed in an electrolyte at 85° C. for 4 h, and the swelling rate was measured and calculated, and the shape retention ability after swelling was observed; the electrolyte solute was 1 mol / L lithium perchlorate trihydrate (CAS: 13453-78-6), and the solvent was 1.2-propylene glycol carbonate (CAS: 108-32-7) and ethylene glycol dimethyl ether (CAS: 110-71-4), and the weight ratio was 1:1; Transverse swelling ratio = (width after immersion in electrolyte / 58) × 100%; Longitudinal swelling rate = (length after immersion in electrolyte / 55) × 100%; Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The swelling tape for lithium batteries prepared in Examples 1 to 6 has strong high temperature resistance and high electrolyte resistance, and expands at a high rate by absorbing electrolyte, can maintain a certain strength and shape in three dimensions, and does not shrink at high temperatures. It is applied to new energy lithium batteries and cylindrical lithium batteries to fill the gap between the battery core and the shell, solving the problems of existing swelling tapes, such as poor high temperature resistance, low expansion rate, failure to form after long-term immersion in electrolyte, low viscosity, and short service life.
[0040] 2) The comparative analysis of the performance of the swelling tape for lithium batteries prepared in combination with Examples 3 and 4-6 shows that the addition of modified silica increases the adhesion between the electrolyte-resistant acrylic coating and the polyurethane swelling coating, prolongs the service life of the swelling tape, and ensures that no residual glue remains when the swelling tape is removed. The present application improves the adsorption performance of the tape by compounding polyurethane resin, polyacrylic resin and modified silica, and solves the technical problem that the existing swelling glue has poor expansion effect in high-temperature electrolyte due to poor temperature resistance. The inventors speculate that the use of polyurethane resin, polyacrylic resin and modified silica for compounding can effectively improve the thermal stability of the electrolyte-resistant acrylic coating, and by improving the temperature resistance of the adhesive film, it essentially avoids battery accidents caused by the shrinkage and expansion of the swelling tape due to high temperature in the prior art.
[0041] 3) The comparative analysis of the performance of the swelling tape for lithium batteries prepared in combination with Example 3 and Comparative Examples 1-2 shows that the polyurethane resin is prepared by mixing a thermoplastic polyurethane resin and a polyurea polyurethane resin in a mass ratio of 7:1. By compounding the thermoplastic polyurethane resin and the polyurea polyurethane resin, the synergistic effect of the two can be achieved, and the performance of the swelling tape can be further improved. On the one hand, this compounding can improve the electrolyte resistance and high temperature resistance of the swelling tape, form a three-dimensional structure with a certain strength, and effectively fill the gap between the battery cell and the shell; on the other hand, this compounding can also make the swelling tape have excellent mechanical properties, and can maintain a high expansion ratio at high temperature without shrinking.
[0042] 4) A comparative analysis of the performance of the swelling tape for lithium batteries prepared in combination with Example 6 and Comparative Example 3 shows that the surface of the unmodified silica still has hydroxyl groups, which easily absorbs moisture in the air and often exhibits phase separation when applied to organic materials. An organic coating layer is formed on the surface of the modified silica, which can effectively reduce the surface energy of the silica, improve the surface properties of the silica, increase the affinity of the silica with organic materials, and enhance the strength, toughness, high temperature resistance, and electrolyte resistance of the swelling tape.
[0043] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. A swelling tape for lithium batteries, characterized in that: The swelling tape comprises, from bottom to top, a release agent coating, a polyurethane swelling coating and an electrolyte-resistant acrylic coating, wherein the release agent coating has a thickness of 0.5-1 μm, the polyurethane swelling coating has a thickness of 10-50 μm, and the electrolyte-resistant acrylic coating has a thickness of 2-10 μm, wherein the electrolyte-resistant acrylic coating is prepared from raw materials, by weight, comprising: 50-100 parts of polyurethane resin, 5-30 parts of polyacrylic resin, 0.5-5 parts of amino resin curing agent, 0.5-10 parts of isocyanate curing agent, and 55-140 parts of solvent.
2. A swelling tape for lithium batteries according to claim 1, characterized in that: The polyurethane resin is prepared by mixing a thermoplastic polyurethane resin and a polyurea polyurethane resin in a mass ratio of 7:
1.
3. A swelling tape for lithium batteries according to claim 1, characterized in that: The isocyanate curing agent is at least one of toluene diisocyanate and diphenylmethane diisocyanate.
4. The swelling tape for lithium battery according to claim 1, characterized in that: The solvent, calculated by weight, includes: 50-110 parts of ethyl acetate and 5-30 parts of N,N-dimethylformamide.
5. The swelling tape for lithium battery according to claim 1, characterized in that: The raw materials for preparing the electrolyte-resistant acrylic coating further include, by weight, 5-6 parts of modified silicon dioxide.
6. A swelling tape for lithium batteries according to claim 5, characterized in that: The preparation method of the modified silicon dioxide comprises the following steps: S61. Dissolve 8 parts of succinic anhydride in 40-50 parts of N,N-dimethylformamide solution according to mass fractions, add 18 parts of γ-aminopropyltriethoxysilane, heat and stir at a water bath temperature of 73° C. for 2-3 hours to obtain a mixed solution A; S62, dissolving 20 parts by mass of silicon dioxide having an average particle size of 20 nm in 50 parts by mass of N,N-dimethylformamide solution to obtain a mixed solution B; S63, adding the mixed solution B dropwise into the mixed solution A, and continuing to stir and react for 3 hours to obtain pretreated silica; S64, the pretreated silica was mixed with 10 parts of 2-methylimidazole and 8 parts of zinc nitrate hexahydrate, and 140 parts of ethanol were added, and ultrasonic polymerization was performed in an 800 W water bath ultrasonic device for 3-4 hours. The obtained product was washed and dried to obtain modified silica.
7. A method for preparing a swelling tape for lithium battery according to any one of claims 1 to 4, characterized in that: The following steps are involved: S71, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S72, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating to control the corona value of the polyurethane swelling coating to be ≥56 dynes; S73, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their weight fractions, and after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, respectively adding the amino resin curing agent and the isocyanate curing agent, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S74. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying. Then, laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared.
8. A swelling tape for lithium batteries according to claim 7, characterized in that: In steps S72 and S74, coating is carried out at a speed of 7-25 m / min, and then entering the oven for drying at the same speed. The temperatures of oven sections 1-8 are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.
9. A method for preparing a swelling tape for lithium battery as claimed in any one of claims 5 to 6, characterized in that: The following steps are involved: S91, dissolving 8 kg of thermoplastic polyurethane resin in 8 kg of N,N-dimethylformamide, and after the thermoplastic polyurethane resin is completely dissolved, adding 0.8 kg of toluene diisocyanate, stirring evenly, to obtain polyurethane glue; S92, applying polyurethane glue to the release surface of the PET single-sided silicon release film, forming a polyurethane swelling coating on the PET single-sided silicon release film after drying, and performing corona treatment on the polyurethane swelling coating to control the corona value of the polyurethane swelling coating to be ≥56 dynes; S93, dissolving the polyurethane resin and the polyacrylic resin in a solvent according to their mass fractions, adding the modified silicon dioxide after the urethane glue polyurethane resin and the polyacrylic resin are completely dissolved, stirring evenly, and finally adding the amino resin curing agent and the isocyanate curing agent respectively, stirring evenly, to obtain an electrolyte-resistant acrylic glue; S94. Apply electrolyte-resistant acrylic glue to the release surface of the PET single-sided silicon release film, and form an electrolyte-resistant acrylic coating on the PET single-sided silicon release film after drying. Then, laminate the electrolyte-resistant acrylic coating and the polyurethane swelling coating. After lamination, peel off the PET single-sided silicon release film, and apply a layer of non-silicone release agent on the peeled polyurethane swelling coating surface. After drying, aging, and stripping, a swelling tape for lithium batteries is prepared.
10. A swelling tape for lithium batteries according to claim 8, characterized in that: In steps S92 and S94, coating is carried out at a speed of 7-25 m / min, and then the surface of the film enters the oven for drying at the same speed. The temperatures of sections 1-8 of the oven are 40°C, 70°C, 90°C, 110°C, 130°C, 130°C, 140°C, and 110°C, respectively.