Decoupling cyclic utilization method for electrolytic manganese sulfide slag

Through the acid-controlled decoupling reaction and saponification extraction technology of ammonium bisulfate and hydrogen peroxide, the problem of the influence of double salts in electrolytic manganese sulfide slag is solved, the efficient separation and diversified utilization of manganese-zinc elements and nickel-cobalt elements are achieved, and the process is simplified process and reduce the accumulation of sulfide slag and the amount of sulfuric acid.

CN118792701APending Publication Date: 2024-10-18BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410815318.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the production process of electrolytic manganese, there are complex salts in the sulfide slag, which affects the utilization efficiency of metals such as nickel, cobalt, and zinc. Moreover, it is difficult to efficiently separate manganese-zinc elements and nickel-cobalt elements with existing technology, resulting in a complicated process flow.

Method used

Ammonium bisulfate and hydrogen peroxide are used to perform an acid-controlled decoupling reaction to separate the nickel-containing cobalt acid leaching residue and the manganese-containing zinc acid leaching solution. The manganese and zinc elements are separated by saponification extraction agent, and then stripping operations and evaporation crystallization are performed to obtain Zinc sulfate and crystallization mother liquor realize diversified utilization of manganese and zinc elements.

Benefits of technology

It effectively separates and recovers manganese-zinc elements and nickel-cobalt elements, simplifies the process flow, reduces sulfide slag accumulation and sulfuric acid consumption, and realizes the diversified utilization of nickel-cobalt-manganese-zinc metal and the recycling of industrial solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792701A_ABST
    Figure CN118792701A_ABST
Patent Text Reader

Abstract

The invention provides a method for decoupling and recycling electrolytic manganese sulfide slag, which comprises the following steps: adding a vulcanizing agent into a manganese sulfate electrolyte for vulcanizing and purifying to obtain sulfide slag and a purified solution, and carrying out manganese electrolysis operation on the purified solution to obtain metal manganese; ammonium bisulfate, water and hydrogen peroxide are added into the vulcanization slag, double salt in the vulcanization slag is decoupled through the ammonium bisulfate, oxidation leaching is conducted on the vulcanization slag through the hydrogen peroxide, and nickel-cobalt-containing acid leaching slag and manganese-zinc-containing acid leaching liquid are obtained through filtering; adding a saponified extraction agent into the manganese-zinc-containing pickle liquor for extraction to obtain a zinc-loaded organic phase; adding sulfuric acid into the zinc-loaded organic phase for reverse extraction to obtain a zinc sulfate solution; and performing evaporative crystallization on the zinc sulfate solution to obtain zinc sulfate. According to the method provided by the invention, the problems of vulcanization slag stacking, large sulfuric acid consumption and the like are effectively solved, the technological process is simplified, diversified utilization is performed on nickel, cobalt, manganese and zinc metals, and direct utilization and cyclic regeneration of industrial solid wastes are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste resource utilization, and particularly relates to a method for decoupling and recycling electrolytic manganese sulfide slag Background Art

[0002] In the process of electrolytic manganese production, most of the manganese sulfate electrolyte is prepared by imported manganese ore or multi-source manganese ore. There is not only a large amount of ammonium sulfate in the solution, but also metal elements such as nickel, cobalt and zinc. Therefore, the sulfidation method is usually used to remove metal elements such as nickel, cobalt and zinc to purify the manganese sulfate electrolyte, but a large amount of sulfide slag is also discarded. The composition of these sulfide slags is complex. In addition to containing sulfides such as MnS, NiS, CoS, and ZnS, there are also a large number of complex salts, such as (NH4)2Me(SO4)2(H2O)6 (Me=Mn, Ni, Co, Zn), and the presence of complex salts directly affects the utilization efficiency of metals such as nickel, cobalt, manganese and zinc in the sulfide slag.

[0003] It can be seen that how to provide a method for decoupling and recycling electrolytic manganese sulfide slag, to control the acid decoupling of the complex salt in the sulfide slag by ammonium bisulfate, to efficiently separate manganese and zinc elements and nickel and cobalt elements, and to simplify the process flow, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0004] The object of the present invention is to provide a method for decoupling and recycling electrolytic manganese sulfide slag to solve at least one of the above technical problems.

[0005] To achieve the above-mentioned object, the first aspect of the present invention provides a method for decoupling and recycling electrolytic manganese sulfide slag, the method comprising the following steps: (1) adding a sulfiding agent to a manganese sulfate electrolyte, separating the solid and the liquid, and obtaining sulfide slag and a purified liquid; (2) subjecting the purified liquid to a manganese electrolysis operation to obtain metallic manganese; (3) adding ammonium bisulfate, water and hydrogen peroxide to the sulfide slag to carry out an acid-controlled decoupling reaction, and filtering to obtain nickel-cobalt-containing acid leaching slag and manganese-containing zinc acid leaching liquid; (4) adding a saponified extractant to the manganese-containing zinc acid leaching liquid to carry out an extraction operation to obtain a zinc-loaded organic phase and a zinc raffinate; the zinc raffinate is reused in the manganese electrolysis operation; (5) adding sulfuric acid to the zinc-loaded organic phase to carry out a stripping operation to obtain a zinc sulfate solution and an unloaded zinc organic phase; (6) subjecting the zinc sulfate solution to evaporation and crystallization to obtain zinc sulfate and a crystallization mother liquor.

[0006] In the first aspect, the step of adding ammonium bisulfate, water and hydrogen peroxide to the sulfide slag to carry out an acid-controlled decoupling reaction, and filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc specifically comprises: adding the sulfide slag and ammonium bisulfate to water, adjusting the temperature to 40 to 80° C., adding hydrogen peroxide, and carrying out an acid-controlled decoupling reaction for 20 to 40 minutes, and then filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc; wherein the solid-liquid ratio of the total amount of the sulfide slag and the ammonium bisulfate added to the water is 1:4 to 1:1.

[0007] In the first aspect, the mass ratio of the ammonium bisulfate to the sulfided slag is 0.6:1 to 1.2:1.

[0008] In the first aspect, the volume ratio of the hydrogen peroxide solution to the water is 0.5% to 1%.

[0009] In the first aspect, in step (1), the sulfiding agent includes at least one of sodium sulfide, ammonium sulfide, manganese sulfide, barium sulfide, sodium thiram and potassium thiram.

[0010] In the first aspect, before performing step (4), the method further includes: adjusting the pH value of the manganese-zinc acid leaching solution to 4.5-5.0.

[0011] In the first aspect, the step of adding a saponified extractant to the manganese-zinc acid leaching solution to perform an extraction operation to obtain a zinc-loaded organic phase and a zinc raffinate specifically includes: mixing P507 and sulfonated kerosene to obtain a native extractant, wherein the volume ratio of P507 to the sulfonated kerosene is 1:9 to 4:6; saponifying the native extractant with sodium hydroxide, wherein the saponification rate is 30% to 60%, to obtain a saponified extractant; adding the saponified extractant to the manganese-zinc acid leaching solution to perform extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase is 1:1 to 3:1, and separating to obtain a zinc-loaded organic phase and a zinc raffinate.

[0012] In the first aspect, in step (5), the volume ratio O / A of the organic phase to the aqueous phase in the stripping operation is 1:10, and the concentration of the sulfuric acid is 2 mol / L.

[0013] In the first aspect, in step (5), the empty organic phase is recycled to the extraction operation.

[0014] In the first aspect, in step (6), the crystallization mother liquor is recycled to the acid-controlled decoupling reaction.

[0015] Beneficial effects:

[0016] The present invention provides a method for decoupling and recycling electrolytic manganese sulfide slag. First, a sulfiding agent is added to a manganese sulfate electrolyte for sulfidation purification to obtain sulfide slag and a purified liquid, and the purified liquid is subjected to manganese electrolysis to obtain metallic manganese; secondly, ammonium bisulfate, water and hydrogen peroxide are added to the sulfide slag, and the double salt in the sulfide slag is decoupled by ammonium bisulfate, and the sulfide slag is oxidized and leached by hydrogen peroxide to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching liquid, so as to efficiently separate manganese and zinc elements from nickel and cobalt elements, and the nickel-cobalt acid leaching slag can be used as a raw material for the short-process preparation of new energy materials. material; then, a saponified extractant is added to the manganese-containing zinc acid leaching solution to perform an extraction operation to separate the manganese element and the zinc element, thereby obtaining a zinc-loaded organic phase and a zinc raffinate, and the zinc raffinate is reused in the manganese electrolysis operation to continue to prepare metallic manganese; finally, sulfuric acid is added to the zinc-loaded organic phase to perform a stripping operation to obtain a zinc sulfate solution and an unloaded zinc organic phase, and the zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor can be subjected to an acid-controlled decoupling reaction together with the sulfide slag, and in addition, the unloaded zinc organic phase can be subjected to an extraction operation together with the manganese-containing zinc acid leaching solution. The present invention uses ammonium bisulfate and hydrogen peroxide as leaching agents, performs acid-controlled decoupling on the sulfided slag after sulfidation purification to separate manganese and zinc elements and nickel and cobalt elements, and sequentially performs zinc extraction, zinc stripping and evaporation crystallization to obtain zinc sulfate, and the manganese sulfate and ammonium sulfate obtained by zinc extraction and separation can be directly recycled to the electrolytic manganese system; the method provided by the present invention effectively solves the problems of sulfided slag stacking and large sulfuric acid consumption, simplifies the process flow, diversifies the utilization of nickel, cobalt, manganese and zinc metals, and realizes the direct utilization and recycling of industrial solid waste.

[0017] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 The process of a method for decoupling and recycling electrolytic manganese sulfide slag in this application Figure 1 ;

[0020] Figure 2 The process of a method for decoupling and recycling electrolytic manganese sulfide slag in this application Figure 2 ;

[0021] Figure 3 is the XRD diagram of the sulfided slag in Example 1 of the present application;

[0022] Figure 4 This is the FT-IR image of the sulfide slag in Example 1 of the present application. DETAILED DESCRIPTION

[0023] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0024] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.

[0026] See also Figure 1 The present application provides a method for decoupling and recycling electrolytic manganese sulfide slag, the method comprising the following steps:

[0027] (1) adding a sulfiding agent to a manganese sulfate electrolyte, separating the solid from the liquid, and obtaining sulfided slag and a purified liquid;

[0028] (2) performing manganese electrolysis on the purified liquid to obtain metallic manganese;

[0029] (3) adding ammonium bisulfate, water and hydrogen peroxide to the sulfided slag to carry out an acid-controlled decoupling reaction, and filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc;

[0030] (4) adding a saponified extractant to the manganese-containing zinc acid leaching solution to perform an extraction operation to obtain a zinc-loaded organic phase and a zinc raffinate; the zinc raffinate is recycled to the manganese electrolysis operation;

[0031] (5) adding sulfuric acid to the zinc-loaded organic phase for stripping to obtain a zinc sulfate solution and an unloaded zinc organic phase;

[0032] (6) Evaporating and crystallizing the zinc sulfate solution to obtain zinc sulfate and a crystallization mother liquor.

[0033] Specifically, the present invention provides a method for decoupling and recycling electrolytic manganese sulfide slag. First, a sulfiding agent is added to a manganese sulfate electrolyte for sulfidation purification to obtain sulfide slag and a purified liquid, and the purified liquid is subjected to manganese electrolysis to obtain metallic manganese; secondly, ammonium bisulfate, water and hydrogen peroxide are added to the sulfide slag, the double salt in the sulfide slag is decoupled by ammonium bisulfate, and the sulfide slag is oxidized and leached by hydrogen peroxide to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching liquid, so as to efficiently separate manganese and zinc elements from nickel and cobalt elements, and the nickel-cobalt acid leaching slag can be used as a short-process preparation method for new energy materials. then, adding a saponified extractant to the manganese-zinc acid leaching solution to perform an extraction operation to separate the manganese element and the zinc element, thereby obtaining a zinc-loaded organic phase and a zinc raffinate, and recycling the zinc raffinate to the manganese electrolysis operation to continue preparing metallic manganese; finally, adding sulfuric acid to the zinc-loaded organic phase to perform a stripping operation to obtain a zinc sulfate solution and an unloaded zinc organic phase, and evaporating and crystallizing the zinc sulfate solution to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor can be subjected to an acid-controlled decoupling reaction together with the sulfide slag, and in addition, the unloaded zinc organic phase can be subjected to an extraction operation together with the manganese-zinc acid leaching solution. The present invention uses ammonium bisulfate and hydrogen peroxide as leaching agents, performs acid-controlled decoupling on the sulfided slag after sulfidation purification to separate manganese and zinc elements and nickel and cobalt elements, and sequentially performs zinc extraction, zinc stripping and evaporation crystallization to obtain zinc sulfate, and the manganese sulfate and ammonium sulfate obtained by zinc extraction and separation can be directly recycled to the electrolytic manganese system; the method provided by the present invention effectively solves the problems of sulfided slag stacking and large sulfuric acid consumption, simplifies the process flow, diversifies the utilization of nickel, cobalt, manganese and zinc metals, and realizes the direct utilization and recycling of industrial solid waste.

[0034] In some possible embodiments, the step of adding ammonium bisulfate, water and hydrogen peroxide to the sulfide slag to carry out an acid-controlled decoupling reaction, and filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc specifically includes: adding the sulfide slag and ammonium bisulfate to water, adjusting the temperature to 40 to 80° C., adding hydrogen peroxide, and carrying out an acid-controlled decoupling reaction for 20 to 40 minutes, and then filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc; wherein the solid-liquid ratio of the total amount of the sulfide slag and the ammonium bisulfate added to the water is 1:4 to 1:1.

[0035] This is because ammonium bisulfate is used as an acid supply agent, water is first added to the ammonium bisulfate and sulfide slag for stirring, and after preliminary dissolution, the temperature is raised to 40-80°C for further dissolution, and ammonium bisulfate is used to decouple the complex salt in the sulfide slag, so that the metal ions and ammonium ions in the complex salt are decoupled and enter the solution, and then hydrogen peroxide is added dropwise for oxidation, so that the manganese and zinc elements and ammonium sulfate are first leached into the acid leaching solution, while the nickel and cobalt elements are not leached into the acid leaching slag.

[0036] In some possible embodiments, the mass ratio of the ammonium bisulfate to the sulfide slag is 0.6:1 to 1.2:1.

[0037] In some possible embodiments, the volume ratio of the hydrogen peroxide solution to the water is 0.5% to 1%.

[0038] In some possible embodiments, in step (1), the sulfiding agent includes at least one of sodium sulfide, ammonium sulfide, manganese sulfide, barium sulfide, sodium thiram and potassium thiram.

[0039] Those skilled in the art can understand that the manganese sulfate electrolyte is first subjected to ion detection to calculate the concentrations of metal ions such as nickel, cobalt, zinc, and manganese, and then the amount of the sulfiding agent to be added is calculated by proportioning, and the sulfiding agent is added to the manganese sulfate electrolyte. The reaction conditions are adjusted so that the manganese ion content in the purified liquid is higher, and the nickel, cobalt, and zinc elements enter the sulfided slag. A combined sulfiding agent formed by mixing an organic sulfiding agent and an inorganic sulfiding agent is preferably used to sulfide and purify the sulfuric acid electrolyte, which can accurately remove metals such as nickel, cobalt, and zinc to form a sulfided slag precipitation for recycling.

[0040] In some possible embodiments, before performing step (4), the method further includes: adjusting the pH value of the manganese-zinc acid leaching solution to 4.5-5.0.

[0041] This is because, before the extraction operation, the pH of the manganese-zinc acid leaching solution needs to be adjusted. The manganese-zinc acid leaching solution contains a large amount of hydrogen ions and is highly acidic, which is not conducive to extraction. Therefore, in order to avoid the introduction of other ions, sulfuric acid or ammonia water can be used to adjust the pH value of the manganese-zinc acid leaching solution to 4.5-5.0 to improve the extraction efficiency.

[0042] In some possible embodiments, the step of adding a saponified extractant to the manganese-zinc acid leaching solution for extraction to obtain a zinc-loaded organic phase and a zinc raffinate specifically includes: mixing P507 and sulfonated kerosene to obtain a native extractant, wherein the volume ratio of P507 to the sulfonated kerosene is 1:9 to 4:6; saponifying the native extractant with sodium hydroxide, wherein the saponification rate is 30% to 60%, to obtain a saponified extractant; adding the saponified extractant to the manganese-zinc acid leaching solution for extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase is 1:1 to 3:1, and separating to obtain a zinc-loaded organic phase and a zinc raffinate.

[0043] Those skilled in the art can understand that adding an extractant to a manganese-zinc acid leaching solution having a pH value of 4.5 to 5.0 and saponifying the extractant with sodium hydroxide can improve the separation effect of zinc and manganese, and zinc enters the zinc-loaded organic phase to participate in the subsequent stripping to purify zinc; while manganese and ammonium sulfate enter the zinc raffinate and are reused in the manganese electrolysis operation. Since the electrolytic manganese system itself needs to contain ammonium sulfate, in this step, manganese sulfate and ammonium sulfate can be directly recycled to the electrolytic manganese system to improve the utilization efficiency of ammonium bisulfate.

[0044] In some possible embodiments, in step (5), the volume ratio O / A of the organic phase to the aqueous phase in the stripping operation is 1:10, and the concentration of the sulfuric acid is 2 mol / L.

[0045] In some possible embodiments, in step (5), the empty organic phase is recycled to the extraction operation.

[0046] This is because, after the zinc-loaded organic phase is stripped with sulfuric acid, the zinc ions enter the aqueous phase and combine with sulfate ions to form a zinc sulfate solution, while the extractant P507 and sulfonated kerosene are present in the organic phase and can be reused in the zinc extraction operation, thereby reducing the use of subsequent extractants.

[0047] In some possible embodiments, in step (6), the crystallization mother liquor is recycled to the acid-controlled decoupling reaction.

[0048] Those skilled in the art can understand that the purity of zinc sulfate obtained after evaporation and crystallization of zinc sulfate solution can reach more than 98%, and the crystallization mother liquor after evaporation and crystallization still contains zinc ions, sulfate ions and other impurity elements. Reusing them in the acid-controlled decoupling reaction can reduce the amount of water used, further purify zinc ions, and improve the recovery efficiency of zinc sulfate.

[0049] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0050] Example 1

[0051] A method for decoupling and recycling electrolytic manganese sulfide slag, specifically comprising the following steps:

[0052] (1) Sulfidation purification: adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0053] (2) manganese electrolysis: subjecting the obtained purified liquid to manganese electrolysis to obtain metallic manganese;

[0054] (3) Acid controlled decoupling: Weigh 10 g of the obtained sulfide slag and 12 g of ammonium bisulfate, add them into 88 mL of water at a solid-liquid ratio of 1:4, raise the temperature to 80°C, add 0.88 ml of hydrogen peroxide, stir and react for 40 min, filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution, and the nickel-cobalt acid leaching slag is centrally processed and can be used as a raw material for the short-process preparation of new energy materials;

[0055] (4) Zinc extraction: the pH value of the manganese-zinc acid leaching solution was adjusted to 5.0, and an extractant formed by mixing P507 saponified with sodium hydroxide and sulfonated kerosene was added to the manganese-zinc acid leaching solution after the pH value was adjusted to carry out extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase was 3:1, and the zinc-loaded organic phase and the zinc raffinate were separated; wherein the volume ratio of P507 to sulfonated kerosene was 4:6, the saponification rate was 60%, and the zinc raffinate was recycled to the manganese electrolysis process;

[0056] (5) Zinc stripping: The obtained zinc-loaded organic phase is stripped with 2 mol / L sulfuric acid at a volume ratio of organic phase to aqueous phase (O / A) = 1:10 to obtain a zinc sulfate solution and an organic phase without zinc, and the organic phase without zinc is recycled to the zinc extraction step;

[0057] (6) Zinc sulfate evaporation and crystallization: The zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor is recycled to the acid control and decoupling process;

[0058] The sulfide slag obtained in step (1) is analyzed and tested. Figure 3 The XRD diagram shows that the sulfide slag after sulfide purification contains manganese sulfide, nickel sulfide, cobalt sulfide and zinc sulfide; Figure 4 The FI-IR diagram shows that the sulfide slag after sulfide purification contains a large amount of complex salts; and the XRF component analysis of the sulfide slag is shown in Table 1, which shows that the sulfide slag mainly contains nickel, cobalt, manganese and zinc metal elements:

[0059] Table 1 XRF composition analysis of sulfide slag

[0060] Elemental composition O S Mn Ni Co Zn content(%) 49.52 29.71 6.18 3.67 7.34 2.93

[0061] The manganese-zinc acid leaching solution in step (2) was subjected to metal ion detection, and the following results were calculated: the manganese recovery rate was 98.2%, the zinc recovery rate was 98.4%, the nickel recovery rate was 1.2%, and the cobalt recovery rate was 1%.

[0062] Example 2

[0063] A method for decoupling and recycling electrolytic manganese sulfide slag, specifically comprising the following steps:

[0064] (1) Sulfidation purification: adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0065] (2) manganese electrolysis: subjecting the obtained purified liquid to manganese electrolysis to obtain metallic manganese;

[0066] (3) Acid controlled decoupling: Weigh 10 g of the obtained sulfide slag, weigh 6 g of ammonium bisulfate, add them into 16 mL of water at a solid-liquid ratio of 1:1, raise the temperature to 40 ° C, add 0.08 ml of hydrogen peroxide, stir and react for 20 min, filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution, and the nickel-cobalt acid leaching slag is centrally processed and can be used as a raw material for the short-process preparation of new energy materials;

[0067] (4) Zinc extraction: the pH value of the manganese-zinc acid leaching solution was adjusted to 4.5, and an extractant formed by mixing P507 saponified with sodium hydroxide and sulfonated kerosene was added to the manganese-zinc acid leaching solution after the pH value was adjusted to perform extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase was 1:1, and the zinc-loaded organic phase and the zinc raffinate were separated; wherein the volume ratio of P507 to sulfonated kerosene was 1:9, the saponification rate was 30%, and the zinc raffinate was recycled to the manganese electrolysis process;

[0068] (5) Zinc stripping: The obtained zinc-loaded organic phase is stripped with 2 mol / L sulfuric acid at a volume ratio of organic phase to aqueous phase (O / A) = 1:10 to obtain a zinc sulfate solution and an organic phase without zinc, and the organic phase without zinc is recycled to the zinc extraction step;

[0069] (6) Zinc sulfate evaporation and crystallization: The zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor is recycled to the acid control and decoupling process;

[0070] The manganese-zinc acid leaching solution in step (2) was subjected to metal ion detection, and the following results were calculated: the manganese recovery rate was 97.5%, the zinc recovery rate was 98.1%, the nickel recovery rate was 0.8%, and the cobalt recovery rate was 0.7%.

[0071] Example 3

[0072] A method for decoupling and recycling electrolytic manganese sulfide slag, specifically comprising the following steps:

[0073] (1) Sulfidation purification: adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0074] (2) manganese electrolysis: subjecting the obtained purified liquid to manganese electrolysis to obtain metallic manganese;

[0075] (3) Acid controlled decoupling: Weigh 10 g of the obtained sulfide slag, weigh 10 g of ammonium bisulfate, add them into 60 mL of water at a solid-liquid ratio of 1:3, raise the temperature to 70 ° C, add 0.54 ml of hydrogen peroxide, stir and react for 30 minutes, filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution, and the nickel-cobalt acid leaching slag is centrally processed and can be used as a raw material for the short-process preparation of new energy materials;

[0076] (4) Zinc extraction: the pH value of the manganese-zinc acid leaching solution was adjusted to 4.8, and an extractant formed by mixing P507 saponified with sodium hydroxide and sulfonated kerosene was added to the manganese-zinc acid leaching solution after the pH value was adjusted to carry out extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase was 2:1, and the zinc-loaded organic phase and the zinc raffinate were separated; wherein the volume ratio of P507 to sulfonated kerosene was 2:8, the saponification rate was 40%, and the zinc raffinate was recycled to the manganese electrolysis process;

[0077] (5) Zinc stripping: The obtained zinc-loaded organic phase is stripped with 2 mol / L sulfuric acid at a volume ratio of organic phase to aqueous phase (O / A) = 1:10 to obtain a zinc sulfate solution and an organic phase without zinc, and the organic phase without zinc is recycled to the zinc extraction step;

[0078] (6) Zinc sulfate evaporation and crystallization: The zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor is recycled to the acid control and decoupling process;

[0079] The manganese-zinc acid leaching solution in step (2) was subjected to metal ion detection, and the following results were calculated: the manganese recovery rate was 99.2%, the zinc recovery rate was 99.1%, the nickel recovery rate was 0.6%, and the cobalt recovery rate was 0.8%.

[0080] Example 4

[0081] A method for decoupling and recycling electrolytic manganese sulfide slag, specifically comprising the following steps:

[0082] (1) Sulfidation purification: adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0083] (2) manganese electrolysis: subjecting the obtained purified liquid to manganese electrolysis to obtain metallic manganese;

[0084] (3) Acid controlled decoupling: Weigh 10 g of the obtained sulfide slag and 8 g of ammonium bisulfate, add them into 36 mL of water at a solid-liquid ratio of 1:2, raise the temperature to 60 ° C, add 0.29 ml of hydrogen peroxide, stir and react for 35 minutes, filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution, and the nickel-cobalt acid leaching slag is centrally processed and can be used as a raw material for the short-process preparation of new energy materials;

[0085] (4) Zinc extraction: the pH value of the manganese-zinc acid leaching solution was adjusted to 4.7, and an extractant formed by mixing P507 saponified with sodium hydroxide and sulfonated kerosene was added to the manganese-zinc acid leaching solution after the pH value was adjusted to carry out extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase was 1.5:1, and the zinc-loaded organic phase and the zinc raffinate were separated; wherein the volume ratio of P507 to sulfonated kerosene was 3:7, the saponification rate was 50%, and the zinc raffinate was recycled to the manganese electrolysis process;

[0086] (5) Zinc stripping: The obtained zinc-loaded organic phase is stripped with 2 mol / L sulfuric acid at a volume ratio of organic phase to aqueous phase (O / A) = 1:10 to obtain a zinc sulfate solution and an organic phase without zinc, and the organic phase without zinc is recycled to the zinc extraction step;

[0087] (6) Zinc sulfate evaporation and crystallization: The zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor is recycled to the acid control and decoupling process;

[0088] The manganese-zinc acid leaching solution in step (2) was subjected to metal ion detection, and the following results were calculated: the manganese recovery rate was 99.3%, the zinc recovery rate was 99.5%, the nickel recovery rate was 0.7%, and the cobalt recovery rate was 0.6%.

[0089] Example 5

[0090] A method for decoupling and recycling electrolytic manganese sulfide slag, specifically comprising the following steps:

[0091] (1) Sulfidation purification: adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0092] (2) manganese electrolysis: subjecting the obtained purified liquid to manganese electrolysis to obtain metallic manganese;

[0093] (3) Acid controlled decoupling: Weigh 10 g of the obtained sulfide slag and 9 g of ammonium bisulfate, add them into 47.5 mL of water at a solid-liquid ratio of 1:2.5, raise the temperature to 50°C, add 0.33 ml of hydrogen peroxide, stir and react for 25 min, filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution, and the nickel-cobalt acid leaching slag is centrally processed and can be used as a raw material for the short-process preparation of new energy materials;

[0094] (4) Zinc extraction: the pH value of the manganese-zinc acid leaching solution was adjusted to 4.9, and an extractant formed by mixing P507 saponified with sodium hydroxide and sulfonated kerosene was added to the manganese-zinc acid leaching solution after the pH value was adjusted to carry out extraction, wherein the volume ratio O / A of the extracted organic phase to the aqueous phase was 1.5:1, and the zinc-loaded organic phase and the zinc raffinate were separated; wherein the volume ratio of P507 to sulfonated kerosene was 2.5:7.5, the saponification rate was 35%, and the zinc raffinate was recycled to the manganese electrolysis process;

[0095] (5) Zinc stripping: The obtained zinc-loaded organic phase is stripped with 2 mol / L sulfuric acid at a volume ratio of organic phase to aqueous phase (O / A) = 1:10 to obtain a zinc sulfate solution and an organic phase without zinc, and the organic phase without zinc is recycled to the zinc extraction step;

[0096] (6) Zinc sulfate evaporation and crystallization: The zinc sulfate solution is evaporated and crystallized to obtain zinc sulfate and a crystallization mother liquor, and the crystallization mother liquor is recycled to the acid control and decoupling process;

[0097] The manganese-zinc acid leaching solution in step (2) was subjected to metal ion detection, and the following results were calculated: the manganese recovery rate was 99.1%, the zinc recovery rate was 99.2%, the nickel recovery rate was 0.8%, and the cobalt recovery rate was 0.9%.

[0098] Comparative Example

[0099] Adding a sulfiding agent to the manganese sulfate electrolyte for sulfidation purification to remove heavy metals such as Ni, Co, and Zn, and obtaining sulfided slag and purified liquid after solid-liquid separation;

[0100] Weigh 10 g of the obtained sulfide slag, measure 30 mL of 2 mol / L sulfuric acid according to a solid-liquid ratio of 1:3, raise the temperature to 80°C, add 0.30 ml of hydrogen peroxide, stir and react for 30 minutes, and filter to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution;

[0101] The ion detection of manganese-zinc acid leaching solution showed that the leaching rates of manganese, zinc, nickel and cobalt were 85.8%, 91.3%, 75.6% and 62.9% respectively.

[0102] In summary, the present invention has at least the following advantages:

[0103] (1) The present invention utilizes ammonium bisulfate and hydrogen peroxide to control the acid decoupling of the double salt in the sulfided slag, and the obtained manganese sulfate and ammonium sulfate are directly circulated to the electrolytic manganese system, thereby avoiding the loss of manganese;

[0104] (2) The present invention uses ammonium bisulfate instead of sulfuric acid as the acid supply agent, which reduces the consumption of sulfuric acid and avoids the generation of H2S. The formed ammonium ions can also enter the electrolytic manganese system for recycling;

[0105] (3) The present invention integrates the sulfidation purification and acid control decoupling processes, thereby realizing the in-situ recycling of manganese in the electrolytic manganese system and the utilization of other metal products;

[0106] (4) The present invention realizes resource utilization of industrial solid waste, simplifies the process flow, and reduces environmental pollution and production costs.

[0107] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0108] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0109] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for decoupling and recycling electrolytic manganese sulfide slag, characterized in that: The method comprises the following steps: (1) adding a sulfiding agent to a manganese sulfate electrolyte, separating the solid from the liquid, and obtaining sulfided slag and a purified liquid; (2) performing manganese electrolysis on the purified liquid to obtain metallic manganese; (3) adding ammonium bisulfate, water and hydrogen peroxide to the sulfided slag to carry out an acid-controlled decoupling reaction, and filtering to obtain an acid leaching slag containing nickel and cobalt and an acid leaching solution containing manganese and zinc; (4) adding a saponified extractant to the manganese-containing zinc acid leaching solution to perform an extraction operation to obtain a zinc-loaded organic phase and a zinc raffinate; the zinc raffinate is recycled to the manganese electrolysis operation; (5) adding sulfuric acid to the zinc-loaded organic phase for stripping to obtain a zinc sulfate solution and an unloaded zinc organic phase; (6) Evaporating and crystallizing the zinc sulfate solution to obtain zinc sulfate and a crystallization mother liquor.

2. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 1, characterized in that: The step of adding ammonium bisulfate, water and hydrogen peroxide to the sulfided slag to perform an acid-controlled decoupling reaction and filtering to obtain the nickel-cobalt-containing acid leaching slag and the manganese-zinc-containing acid leaching solution specifically comprises: The sulfide slag and ammonium bisulfate are added into water, the temperature is adjusted to 40-80° C., hydrogen peroxide is added, and the acid-controlled decoupling reaction is performed for 20-40 minutes, followed by filtering to obtain nickel-cobalt acid leaching slag and manganese-zinc acid leaching solution; Wherein, the solid-liquid ratio of the total amount of the sulfide slag and the ammonium bisulfate added to the water is 1:4 to 1:

1.

3. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 2, characterized in that: The mass ratio of the ammonium bisulfate to the sulfide slag is 0.6:1 to 1.2:

1.

4. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 3, characterized in that: The volume ratio of the hydrogen peroxide solution to the water is 0.5% to 1%.

5. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 1, characterized in that: In step (1), the sulfiding agent includes at least one of sodium sulfide, ammonium sulfide, manganese sulfide, barium sulfide, sodium thiram and potassium thiram.

6. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 1, characterized in that: Before performing step (4), the method further includes: adjusting the pH value of the manganese-zinc acid leaching solution to 4.5-5.

0.

7. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 6, characterized in that: The step of adding a saponified extractant to the manganese-zinc acid leaching solution to perform an extraction operation to obtain a zinc-loaded organic phase and a zinc raffinate specifically comprises: Mixing P507 and sulfonated kerosene to obtain a primary extractant, wherein the volume ratio of the P507 to the sulfonated kerosene is 1:9 to 4:6; The raw extractant is subjected to saponification treatment with sodium hydroxide, with a saponification rate of 30% to 60%, to obtain a saponified extractant; The saponification extractant is added to the manganese-zinc acid leaching solution to perform extraction, wherein the volume ratio O / A of the extraction organic phase to the aqueous phase is 1:1 to 3:1, and the zinc-loaded organic phase and the zinc raffinate are separated.

8. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 1, characterized in that: In step (5), the volume ratio O / A of the organic phase to the aqueous phase in the stripping operation is 1:10, and the concentration of the sulfuric acid is 2 mol / L.

9. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 8, characterized in that: In step (5), the empty organic phase is recycled to the extraction operation.

10. The method for decoupling and recycling electrolytic manganese sulfide slag according to claim 1, characterized in that: In step (6), the crystallization mother liquor is recycled into the acid-controlled decoupling reaction.