Preparation method and application of TOPCon battery mask layer

The thermal oxidation method is used to generate a SiO2 mask layer at a specific temperature, which solves the problems of poor density and corrosion resistance of the SiO2 mask layer prepared by the PECVD method, and significantly improves the efficiency and yield of the cell.

CN118800829AInactive Publication Date: 2024-10-18DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410807192.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the SiO2 mask layer prepared by the PECVD method has poor density and corrosion resistance, resulting in low yield and efficiency of the battery cells.

Method used

Thermal oxidation method is used to pass O2 and N2 into the cell at 800℃-1000℃ to generate a SiO2 mask layer with better density and corrosion resistance. It is evacuated through a high temperature resistant furnace tube to improve the uniformity of the diaphragm. .

Benefits of technology

Significantly improves the density and corrosion resistance of the SiO2 mask layer, and improves the efficiency yield and passivation performance of the cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800829A_ABST
    Figure CN118800829A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a TOPCon cell mask layer, and relates to the technical field of solar cells, and the preparation method of the mask layer comprises the following steps: employing O2 and N2 to prepare a SiO2 mask layer on a cell through a thermal oxidation method; wherein the temperature of the thermal oxidation method is 800-1000 DEG C. The technical problem that the SiO2 mask layer is poor in compactness and corrosion resistance when the SiO2 mask layer is prepared through a PECVD method in the prior art is solved, and the technical effects that the compactness and corrosion resistance of the SiO2 mask layer are remarkably improved, the protection effect of the Poly layer is improved, and the passivation performance and the electric leakage proportion of a battery piece are effectively improved are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a preparation method of a TOPCon cell mask layer and application thereof. Background Art

[0002] TOPCon (Tunnel Oxide Passivating Contacts) cells use PECVD (Plasma Enhanced Chemical Vapor Deposition) to prepare Poly (polycrystalline silicon layer). Before the process reaction is completed, N2O and SiH4 will be introduced for ionization to generate SiO2, which is the mask layer. Its main function is to protect the amorphous silicon layer from being corroded by the alkaline tank in the subsequent cleaning process. The existing technology uses PECVD to prepare the SiO2 mask layer, and its film density and corrosion resistance are poor, which will reduce the yield and efficiency of the battery cell.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] One of the purposes of the present invention is to provide a method for preparing a TOPCon battery mask layer, which can significantly improve the density and corrosion resistance of the SiO2 mask layer, effectively improve the uniformity within the SiO2 membrane, and help improve the efficiency and yield of the battery cell.

[0005] The second object of the present invention is to provide an application of a method for preparing a TOPCon battery mask layer, which is beneficial to improving the passivation performance and improving the battery efficiency.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0007] In a first aspect, a method for preparing a TOPCon battery mask layer comprises the following steps:

[0008] A SiO2 mask layer is prepared on the cell by thermal oxidation using O2 and N2;

[0009] The temperature of the thermal oxidation method is 800°C-1000°C.

[0010] Furthermore, the process parameters of the thermal oxidation method are as follows:

[0011] The O2 flow rate is 10slm-20slm; and / or, the N2 flow rate is 3slm-5slm.

[0012] Furthermore, the thermal oxidation method is carried out for 5 minutes to 20 minutes.

[0013] Furthermore, the equipment used in the thermal oxidation method includes a high temperature resistant furnace tube.

[0014] Furthermore, the thermal oxidation method further includes a step of evacuating the high temperature resistant furnace tube.

[0015] Further, the evacuation process comprises the following steps:

[0016] First, introduce N2 into the furnace tube, and then evacuate the furnace tube;

[0017] Preferably, the flow rate of N2 is 10slm-30slm;

[0018] Preferably, the evacuation pressure is 200 mbar-300 mbar.

[0019] Furthermore, the cell comprises a cell on which a doped amorphous silicon film is deposited.

[0020] Furthermore, the mask layer is prepared to have a thickness of 10nm-20nm.

[0021] In a second aspect, a method for preparing a mask layer as described in any one of the above items is used in the production of TOPCon batteries.

[0022] Furthermore, the thickness of the polysilicon film of the TOPCon cell is 100nm-150nm.

[0023] Compared with the prior art, the present invention has at least the following beneficial effects:

[0024] The method for preparing a TOPCon battery mask layer provided by the present invention adopts a thermal oxidation method to prepare a SiO2 mask layer, thereby solving the technical problem that when the SiO2 mask layer is prepared by a PECVD method in the prior art, the SiO2 mask layer has poor compactness and poor corrosion resistance. At a specific temperature of 800°C-1000°C in the thermal oxidation method, O2 and N2 are introduced to react on the battery cell to generate a SiO2 mask layer with better compactness and better corrosion resistance, thereby effectively improving the uniformity within the SiO2 diaphragm, thereby being able to improve the protection effect of the Poly layer, which is beneficial to improving the efficiency and yield of the battery cell.

[0025] The application of the preparation method of the TOPCon battery mask layer provided by the present invention is beneficial to improving the passivation performance and improving the battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A flow chart of preparing a TOPCon battery mask layer provided in one embodiment of the present invention;

[0028] Figure 2 It is a flow chart of preparing the TOPCon battery mask layer in the prior art;

[0029] Figure 3 This is a schematic diagram of the structure of the TOPCon battery provided by the present invention.

[0030] Icon: 1-Si substrate; 2-tunneling layer; 3-polysilicon layer; 4-SiO2 mask layer. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] According to a first aspect of the present invention, a method for preparing a TOPCon battery mask layer is provided, comprising the following steps:

[0033] A SiO2 mask layer is prepared on the cell by thermal oxidation using O2 and N2;

[0034] Among them, the temperature of the thermal oxidation method is 800℃-1000℃.

[0035] The method for preparing the TOPCon battery mask layer provided by the present invention adopts a thermal oxidation method to prepare a SiO2 mask layer on an amorphous silicon layer (see Figure 1 ), which solves the problem of using PECVD method to prepare SiO2 mask layer in the prior art (see Figure 2 ) (by ionizing N2O and SiH4 to generate a SiO2 mask layer), the SiO2 mask layer has technical problems of poor density and poor corrosion resistance. Under the specific temperature of 800℃-1000℃ of the thermal oxidation method, O2 and N2 are introduced to react on the battery cell to generate a SiO2 mask layer with better density and better corrosion resistance, which effectively improves the uniformity within the SiO2 membrane, thereby improving the protection effect of the Poly layer, which is beneficial to improving the efficiency and yield of the battery cell.

[0036] In the present invention, typical but non-limiting temperatures of the thermal oxidation method are, for example, 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, and 1000°C. The appropriate temperature of the thermal oxidation method can ensure the formation of a SiO2 mask layer with better density and better corrosion resistance on the battery cell (using a silicon substrate), and can effectively improve the uniformity within the SiO2 film; if the temperature of the thermal oxidation method is too high, the oxide film formation rate will be faster, resulting in poor density; if the temperature of the thermal oxidation method is too low, the oxide film formation rate will be slower, resulting in lower production capacity.

[0037] In a preferred embodiment, the process parameters of the thermal oxidation method are as follows:

[0038] The flow rate of O2 may be 10 slm-20 slm, for example, 10 slm, 11 slm, 12 slm, 13 slm, 14 slm, 15 slm, 16 slm, 17 slm, 18 slm, 19 slm, 20 slm, but is not limited thereto;

[0039] And / or, the flow rate of N2 can be 3slm-5slm, for example, 3slm, 3.2slm, 3.4slm, 3.6slm, 3.8slm, 4slm, 4.2slm, 4.4slm, 4.6slm, 4.8slm, 5slm, but not limited to this.

[0040] The process parameters of the thermal oxidation method in the present invention are more conducive to further improving the compactness and corrosion resistance of the SiO2 mask layer, and are more conducive to further improving the uniformity within the SiO2 film.

[0041] In a preferred embodiment, the duration of the thermal oxidation method can be 5min-20min, and its typical but non-limiting duration is, for example, 5min, 6min, 7min, 8min, 9min, 10min, 12min, 14min, 16min, 18min, and 20min, which is more conducive to further improving the generation effect of the SiO2 mask layer; if the duration of the thermal oxidation method is too short, the oxide film formation rate will be faster, resulting in poor density; if the duration of the thermal oxidation method is too long, the oxide film formation rate will be slower, resulting in lower production capacity.

[0042] In summary, the various parameters of the thermal oxidation method in the present invention can cooperate with each other, thereby significantly improving the density and corrosion resistance of the SiO2 mask layer, and fully improving the uniformity within the SiO2 membrane, which is extremely beneficial to improving the efficiency and yield of the battery cell.

[0043] In a preferred embodiment, the equipment used in the thermal oxidation method includes but is not limited to high temperature resistant furnace tubes.

[0044] In the present invention, the battery cell enters a high temperature resistant furnace tube, the temperature in the furnace is set to 800°C-1000°C, the furnace tube can be evacuated, leak tested and kept at a constant temperature, and then O2 and N2 are introduced into the furnace tube for high temperature reaction, thereby generating a SiO2 mask layer on the battery cell.

[0045] In a preferred embodiment, the solar cells used in the present invention include but are not limited to solar cells deposited with doped amorphous silicon thin films.

[0046] In the present invention, SiH4, H2 and PH3 gases can be used for ionization to deposit doped amorphous silicon film; wherein, the flow rate of SiH4 can be 1000sccm-4000sccm, for example, it can be 1000sccm, 2000sccm, 3000sccm, 4000sccm, but not limited to this; the flow rate of H2 can be 4000sccm-6000sccm, for example, it can be 4000sccm, 5000sccm, 6000sccm, but not limited to this; the flow rate of PH3 can be 300sccm-700sccm, for example, it can be 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, but not limited to this; the thickness of the deposited doped amorphous silicon film can be 100nm-150nm, and its typical but non-limiting thickness is, for example, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm.

[0047] In a preferred embodiment, the thermal oxidation method further includes a step of evacuating the high temperature resistant furnace tube.

[0048] In a preferred embodiment, the evacuation process comprises the following steps:

[0049] First, introduce N2 into the furnace tube, and then evacuate the furnace tube;

[0050] The flow rate of N2 may be 10 slm-30 slm, for example, 10 slm, 12 slm, 14 slm, 16 slm, 18 slm, 20 slm, 22 slm, 24 slm, 26 slm, 28 slm, 30 slm, but is not limited thereto;

[0051] The evacuation pressure may be 200 mbar-300 mbar, for example, 200 mbar, 220 mbar, 240 mbar, 260 mbar, 280 mbar, 300 mbar, but is not limited thereto.

[0052] In a preferred embodiment, the preparation thickness of the mask layer of the present invention can be 10nm-20nm, for example, it can be 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, which is more conducive to further improving the protection effect of the Poly layer and further improving the passivation performance and leakage ratio of the battery cell.

[0053] A TOPCon battery, the structure is shown in Figure 3 , comprising a Si substrate 1, a tunneling layer 2 on the Si substrate 1, a polysilicon layer 3 on the tunneling layer 2, and a SiO2 mask layer 4 on the polysilicon layer 3, and the corresponding preparation method comprises the following steps:

[0054] Step 1: The Poly process starts to run, the cell (Si substrate 1 and tunneling layer 2 deposited thereon) enters the PECVD furnace tube, the chamber starts to be purged and heated to the process set temperature, which is 400-500°C;

[0055] Step 2: Purge the PECVD furnace tube with nitrogen and perform evacuation and leak detection;

[0056] Step 3: SiH4, H2 and PH3 gases are introduced for ionization, thereby depositing a doped amorphous silicon film on the cell, and subsequently forming a polycrystalline silicon layer 3 with a thickness of 100-150nm;

[0057] Among them, SiH4 flow rate is 1000sccm-4000sccm; H2 flow rate is 4000sccm-6000sccm; PH3 flow rate is 300sccm-700sccm;

[0058] Step 4: Cool down, evacuate, pressurize and unload the boat;

[0059] Step 5: The battery cell enters the high temperature resistant furnace tube, and the temperature in the furnace rises to the process setting temperature, which is 800-1000℃;

[0060] Step 6: Evacuate, leak test and maintain constant temperature on the furnace tube;

[0061] Step 7: introducing O2 and N2 to react at 800-1000°C (thermal oxidation method), thereby forming a SiO2 mask layer 4 on the cell with a thickness of 10nm-20nm;

[0062] The process parameters of the reaction are: O2 flow rate 3slm-20slm; N2 flow rate 3slm-5slm; reaction time 5min-20min;

[0063] Step 8: Evacuate the furnace tube with N2;

[0064] Among them, the vacuum treatment parameters are: N2 10slm-30slm; pressure 200mbar-300mbar;

[0065] Step 9: After N2 evacuation treatment, annealing treatment is performed to activate the amorphous silicon layer;

[0066] The annealing temperature is 800°C-1000°C and the time is 30min-60min.

[0067] Step 10: After annealing, cool down the furnace tube, break the vacuum, and take out the boat.

[0068] According to a second aspect of the present invention, there is provided an application of any one of the methods for preparing a mask layer in TOPCon cell production.

[0069] The application of the preparation method of the TOPCon battery mask layer provided by the present invention is beneficial to improving the passivation performance and improving the battery efficiency.

[0070] In a preferred embodiment, the thickness of the polysilicon film of the TOPCon cell may be 100 nm-150 nm, and typical but non-limiting thicknesses thereof are, for example, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, and 150 nm.

[0071] In the present invention, the doped amorphous silicon film can be transformed into a polycrystalline silicon film through annealing treatment; wherein, the temperature of the annealing treatment can be 800℃-1000℃, for example, it can be 800℃, 820℃, 840℃, 860℃, 880℃, 900℃, 920℃, 940℃, 960℃, 980℃, 1000℃, but not limited to this, which is more conducive to improving the formation effect of the polycrystalline silicon film; the annealing treatment time can be 30min-60min, for example, it can be 30min, 32min, 34min, 36min, 38min, 40min, 45min, 50min, 55min, 60min, but not limited to this, which is more conducive to further improving the formation effect of the polycrystalline silicon film.

[0072] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0073] Example 1

[0074] A method for preparing a TOPCon battery mask layer comprises the following steps:

[0075] Step 1: The Poly process starts running, the cell (Si substrate and the tunneling layer deposited on it) enters the PECVD furnace tube, the chamber starts to be purged and heated to the process set temperature, which is 450°C;

[0076] Step 2: Purge the PECVD furnace tube with nitrogen and perform evacuation and leak detection;

[0077] Step 3: SiH4, H2 and PH3 gases are introduced for ionization, thereby depositing a doped amorphous silicon film on the cell with a thickness of 130nm;

[0078] Among them, SiH4 flow rate is 2450sccm; H2 flow rate is 5000sccm; PH3 flow rate is 640sccm;

[0079] Step 4: Cool down, evacuate, pressurize and unload the boat;

[0080] Step 5: The battery cell enters the high temperature resistant furnace tube, and the temperature in the furnace rises to the process set temperature, which is 900°C;

[0081] Step 6: Evacuate, leak test and maintain constant temperature on the furnace tube;

[0082] Step 7: O2 and N2 are introduced to react at 900°C (thermal oxidation method), thereby forming a SiO2 mask layer on the cell with a thickness of 15nm;

[0083] The process parameters of the reaction are: O2 flow rate 3slm; N2 flow rate 5slm; reaction time 15min;

[0084] Step 8: Evacuate the furnace tube with N2;

[0085] The vacuum treatment parameters are: N2 20slm; pressure 250mbar;

[0086] Step 9: After N2 evacuation treatment, annealing treatment is performed to activate the amorphous silicon layer;

[0087] The annealing temperature is 900°C and the time is 45 min.

[0088] Step 10: After annealing, cool down the furnace tube, break the vacuum, and take out the boat.

[0089] Example 2

[0090] The difference between this embodiment and embodiment 1 is that the reaction temperature in step 7 is 800° C., thereby forming a SiO2 mask layer on the cell;

[0091] The remaining steps and process parameters are the same as those in Example 1.

[0092] Example 3

[0093] The difference between this embodiment and embodiment 1 is that the reaction temperature in step 7 is 1000° C., thereby forming a SiO2 mask layer on the cell;

[0094] The remaining steps and process parameters are the same as those in Example 1.

[0095] Example 4

[0096] The difference between this embodiment and embodiment 1 is that the process parameters of the reaction in step 7 are: O2 flow rate 5slm; N2 flow rate 5slm; reaction time 8min; thereby generating a SiO2 mask layer on the cell with a thickness of 10nm;

[0097] The remaining steps and process parameters are the same as those in Example 1.

[0098] Example 5

[0099] The difference between this embodiment and embodiment 1 is that the process parameters of the reaction in step 7 are: O2 flow rate 5slm; N2 flow rate 3slm; reaction time 20min; thereby generating a SiO2 mask layer on the cell with a thickness of 20nm;

[0100] The remaining steps and process parameters are the same as those in Example 1.

[0101] Example 6

[0102] The difference between this embodiment and embodiment 1 is that the reaction time in step 7 is 5 minutes; thereby a SiO2 mask layer is generated on the cell;

[0103] The remaining steps and process parameters are the same as those in Example 1.

[0104] Example 7

[0105] The difference between this embodiment and embodiment 1 is that the reaction time in step 7 is 20 minutes; thereby a SiO2 mask layer is generated on the cell;

[0106] The remaining steps and process parameters are the same as those in Example 1.

[0107] Comparative Example 1

[0108] The difference between this comparative example and Example 1 is that in step 7, this comparative example adopts PECVD method to prepare SiO2 mask layer (by ionizing N2O and SiH4 to generate SiO2 mask layer);

[0109] The parameters of the PECVD method are as follows: N2O flow rate 9800sccm; SiH4 flow rate 2000sccm; reaction time 35s;

[0110] The remaining steps and process parameters are the same as those in Example 1.

[0111] Compared with Example 1, the defect of the SiO2 mask layer prepared in this comparative example is that the density and corrosion resistance of the mask layer are poor, which will reduce the yield and efficiency of the battery cell.

[0112] Comparative Example 2

[0113] The difference between this comparative example and Example 1 is that the reaction temperature in step 7 is 750°C;

[0114] The remaining steps and process parameters are the same as those in Example 1.

[0115] Compared with Example 1, the defect of the SiO2 mask layer prepared in this comparative example is that the film layer is relatively thin and has poor corrosion resistance.

[0116] Comparative Example 3

[0117] The difference between this comparative example and Example 1 is that the reaction temperature in step 7 is 1050°C;

[0118] The remaining steps and process parameters are the same as those in Example 1.

[0119] Compared with Example 1, the defect of the SiO2 mask layer prepared in this comparative example is that the film forming rate is fast, resulting in poor density.

[0120] Experimental example

[0121] According to the test items in Table 1, the TOPCon cells and their SiO2 mask layers prepared in Examples 1-7 and Comparative Examples 1-3 were tested. The test results are shown in Table 1.

[0122] Test method: Use the ellipsoid offset method to test the film thickness;

[0123] UOC (open circuit voltage) and Irev (leakage current) are tested according to industry standard methods.

[0124] It should be noted that the compactness is characterized by UOC (open circuit voltage). Good compactness means good passivation effect and high UOC. The corrosion resistance is characterized by Irev (leakage current). Poor corrosion resistance means high leakage current.

[0125] Table 1

[0126]

[0127] As can be seen from Table 1, the present invention adopts a thermal oxidation method to prepare a SiO2 mask layer. Under the coordinated cooperation of specific process parameters of the thermal oxidation method, a SiO2 mask layer with better density and better corrosion resistance is generated on the battery cell, which effectively improves the uniformity within the SiO2 membrane, thereby improving the protection effect of the Poly layer, which is beneficial to improving the efficiency and yield of the battery cell.

[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a TOPCon battery mask layer, characterized in that: The following steps are involved: A SiO2 mask layer is prepared on the cell by thermal oxidation using O2 and N2; The temperature of the thermal oxidation method is 800°C-1000°C.

2. The preparation method according to claim 1, characterized in that: The process parameters of the thermal oxidation method are as follows: The O2 flow rate is 10slm-20slm; and / or, the N2 flow rate is 3slm-5slm.

3. The preparation method according to claim 1 or 2, characterized in that: The duration of the thermal oxidation method is 5 min to 20 min.

4. The preparation method according to claim 1, characterized in that: The equipment used in the thermal oxidation method includes a high temperature resistant furnace tube.

5. The preparation method according to claim 4, characterized in that: The thermal oxidation method further includes a step of evacuating the high temperature resistant furnace tube.

6. The preparation method according to claim 5, characterized in that: The evacuation process comprises the following steps: First, introduce N2 into the furnace tube, and then evacuate the furnace tube; Preferably, the flow rate of N2 is 10slm-30slm; Preferably, the evacuation pressure is 200 mbar-300 mbar.

7. The preparation method according to claim 1, characterized in that: The cell comprises a cell on which a doped amorphous silicon film is deposited.

8. The preparation method according to claim 1, characterized in that: The mask layer is prepared to have a thickness of 10nm-20nm.

9. Application of the method for preparing a mask layer according to any one of claims 1 to 8 in TOPCon battery production.

10. The use according to claim 9, characterized in that: The thickness of the polysilicon film of the TOPCon cell is 100nm-150nm.

Citation Information

Patent Citations

  • N-type passivated contact battery and preparation method thereof

    CN111640823A

  • Solar cell and preparation method and application thereof

    CN114792744A

  • P-type passivation contact cell preparation method and passivation contact cell

    CN115000246A

  • Method for preparing boron-doped selective emitter battery

    WO2023045279A1

  • Solar cell and preparation method therefor, and photovoltaic system

    WO2023213088A1