Preparation method of passivation contact solar cell and passivation contact solar cell
By adjusting the arrangement sequence and stacking structure of silicon wafers, the problems of uneven thickness of tunnel oxide layer and difference in oxygen concentration are solved, the yield rate and passivation performance of passivated contact solar cells are improved, and the process is simplified and the cost is reduced. reduce.
Patent Information
- Application Number
- CN202411143083.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-18
AI Technical Summary
In the preparation process of passivated contact solar cells, due to the uneven thickness of the tunnel oxide layer and the difference in oxygen concentration, the passivation performance is poor and the yield is low, leaving room for process improvement.
By adjusting the arrangement of the silicon wafers in the quartz boat, and using thermal oxygen technology and chemical vapor deposition technology, the tunnel oxide layer, barrier layer and doped polysilicon layer are formed to ensure that the thickness of the tunnel oxide layer and barrier layer match, and the needle is enhanced. The hole effect and the diffusion ability of doping elements prevent doping elements from damaging the tunnel oxide layer.
It effectively improves the yield rate and passivation performance of passivated contact solar cells, simplifies the process flow, expands the process window, reduces production difficulty and cost, and is suitable for mass production.
Smart Images

Figure CN118800841A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a passivation contact solar cell and a passivation contact solar cell. Background Art
[0002] For passivated contact solar cells, a good match between the tunnel oxide layer and the doped polysilicon layer is the key to the passivated contact solar cells to obtain excellent passivation performance and contact performance. The quality of the tunnel oxide layer will directly affect the degree of matching between it and the doped polysilicon layer. At present, in the process of preparing the tunnel oxide layer by carrying silicon wafers on a quartz boat, since the uniformity of the high-temperature epitaxial growth of the tunnel oxide layer is affected by the temperature field and the gas field, the heat will be partially absorbed in the area of the silicon wafer near the bottom of the quartz boat, and due to the obstruction of the quartz boat, the oxygen concentration in the area of the silicon wafer near the bottom of the quartz boat is also lower than the oxygen concentration in the area near the top of the quartz boat. On the whole, the tunnel oxide layer of the silicon wafer gradually becomes thinner from the top to the bottom of the quartz boat, resulting in a low yield of the passivated contact solar cells with excellent passivation contact performance. There is still a relatively large room for process improvement in passivated contact solar cells. Summary of the invention
[0003] In view of this, the present invention provides a method for preparing a passivated contact solar cell and a passivated contact solar cell, which improves the preparation process of the passivated contact solar cell and effectively improves the yield rate of the passivated contact solar cell with excellent passivation contact performance.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] In a first aspect, the present invention provides a method for preparing a passivated contact solar cell, comprising:
[0006] Step 1, placing the silicon wafer in a quartz boat;
[0007] Step 2: preparing a tunneling oxide layer on the first main surface of the silicon wafer by a thermal oxidation process;
[0008] Step 3, controlling the wafer inserting machine to change the direction of the silicon wafer in the quartz boat;
[0009] Step 4, sequentially stacking a first intrinsic polysilicon layer, a barrier layer, and a second intrinsic polysilicon layer on the tunnel oxide layer by chemical vapor deposition;
[0010] Step 5: Perform a doping element thermal diffusion activation process on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer to form a first doped polysilicon layer and a second doped polysilicon layer.
[0011] In a second aspect, an embodiment of the present invention provides a passivated contact solar cell, comprising: a silicon wafer, a tunneling oxide layer, a first doped polysilicon layer, a barrier layer, and a second doped polysilicon layer stacked on a first main surface of the silicon wafer, wherein:
[0012] The type of doping element included in the first doped polysilicon layer is consistent with the type of doping element included in the second doped polysilicon layer;
[0013] The doping concentration of the first doped polysilicon layer is lower than the doping concentration of the second doped polysilicon layer.
[0014] The technical solution of the first aspect of the above invention has the following advantages or beneficial effects:
[0015] The preparation method provided by the embodiment of the present invention adjusts the arrangement order of the silicon wafer after preparing the tunneling oxide layer, and then sequentially stacks a first intrinsic polysilicon layer, a barrier layer and a second intrinsic polysilicon layer on the adjusted silicon wafer, so that a thicker barrier layer is formed on the thinner area of the tunneling oxide layer on the silicon wafer, and a thinner barrier layer is formed on the thicker area with the tunneling oxide layer, that is, by matching the thickness of the tunneling oxide layer with the thickness of the barrier layer, the thicker area of the tunneling oxide layer is matched with the thinner barrier layer, so that the ability of the barrier layer to block doped elements is reduced, so that the tunneling oxide layer can produce a sufficient pinhole effect, and the thinner area of the tunneling oxide layer is matched with the thicker barrier layer, so as to improve the ability to block the diffusion of doped elements, avoid the doped elements from destroying the tunneling oxide layer, improve the preparation process of the passivation contact solar cell, and effectively improve the yield of the passivation contact solar cell with excellent passivation contact performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 1 is a schematic diagram of the main process of a method for preparing a passivated contact solar cell according to an embodiment of the present invention;
[0017] Figure 2 is a method according to an embodiment of the present invention corresponding to Figure 1 Schematic diagram of the structural changes of the solar cell in the process shown;
[0018] Figure 3 is a method according to an embodiment of the present invention corresponding to Figure 1 The schematic diagram of the change of the direction of the silicon wafer in step S103 is shown;
[0019] Figure 4 is a schematic diagram of the main process of another method for preparing a passivated contact solar cell according to an embodiment of the present invention;
[0020] Figure 5 1 is a partial structural schematic diagram of a passivated contact solar cell according to an embodiment of the present invention.
[0021] Description of reference numerals:
[0022] 10-silicon wafer; 20-tunneling oxide layer; 30-first doped polysilicon layer; 40-barrier layer; 50-second doped polysilicon layer; 60-emitter of PN junction; 70-aluminum oxide film layer; 80-front passivation layer; 90-back passivation layer; 100-metal electrode. DETAILED DESCRIPTION
[0023] For passivated contact solar cells, a good match between the tunnel oxide layer and the doping layer is the key to obtaining excellent passivation performance. When the doping element penetrates the tunnel oxide layer into the silicon substrate, the tunnel oxide layer is destroyed, its blocking effect on minority carriers is significantly weakened, and the tunnel passivation basically fails. The potential energy barrier between the intrinsic doping layer of a small amount of doping elements formed on the surface of the silicon substrate and the doped polysilicon layer stacked on the outside of the tunnel oxide layer is reduced. For example, for phosphorus doping elements, an intrinsic doping layer N is formed on the surface of the silicon substrate. + -Si, the doped polysilicon layer stacked outside the tunnel oxide layer is N ++ -Si, after the tunnel oxide layer is destroyed, N + -Si and N ++ -Si has a smaller potential energy barrier, the separation effect of high-low junction electron-hole pairs is weakened, and field passivation is basically ineffective. The subsequent hydrogen passivation repair of dangling bonds cannot make up for the decrease in passivation. When there are few doping elements entering the silicon matrix, for example, for phosphorus doping, N + When the doping concentration of -Si is low, although the field passivation effect can be guaranteed, the majority carriers cannot easily pass through the tunneling oxide layer, resulting in limited tunneling passivation.
[0024] In the actual production of passivated contact solar cells, as described in the background technology, the thickness of the tunneling oxide layer formed in different areas of the silicon wafer placed in the quartz boat is different, that is, the closer the silicon wafer is to the bottom of the quartz boat, the thinner the thickness of the tunneling oxide layer formed therein is, and the closer the silicon wafer is to the top of the quartz boat, the thicker the thickness of the tunneling oxide layer formed therein is. This makes the thickness of the tunneling oxide layer formed on the silicon wafer inconsistent, resulting in the subsequent doping layer formation process, the silicon wafer either fails to achieve the tunneling passivation effect, or the tunneling oxide layer is damaged.
[0025] In order to solve the above problems existing in the existing process, the embodiments of the present invention provide a novel method for preparing a passivated contact solar cell and a passivated contact solar cell.
[0026] The type of the doping element involved in the embodiments of the present invention is generally N-type or P-type.
[0027] The doping concentration involved in the embodiments of the present invention generally refers to the concentration of the doping element contained in the doping layer after the doping element is activated.
[0028] Regarding the formation of another structure on a structure involved in the embodiments of the present invention, the two structures may be in direct or indirect contact. That is, the other structure may be directly formed on the structure and directly contact the structure. In addition, the other structure may be first formed on the structure, and then the other structure may be formed on the other structure, that is, the structure is in indirect contact with the other structure.
[0029] It is worth noting that the terms "first", "second", etc. included in the embodiments of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific number or sequence. It should be understood that the terms used in this way can be interchangeable under appropriate circumstances, and this is merely a way of distinguishing objects with the same attributes when describing them in the embodiments of the present invention.
[0030] Embodiments of the present invention Figure 1 A schematic diagram showing the main process of the method for preparing a passivated contact solar cell provided by an embodiment of the present invention is shown.
[0031] like Figure 1 As shown, the method for preparing a passivated contact solar cell provided by an embodiment of the present invention may include the following steps:
[0032] Step S101: placing a silicon wafer in a quartz boat;
[0033] The silicon wafer involved in the embodiment of the present invention may be an N-type silicon wafer or a P-type silicon wafer. Preferably, the silicon wafer involved in the embodiment of the present invention is an N-type silicon wafer.
[0034] The silicon wafer can be placed in the quartz boat directly by using existing technical processes, for example, the silicon wafer can be automatically inserted into the quartz boat by a wafer inserting machine.
[0035] Step S102: preparing a tunneling oxide layer 20 on the first main surface of the silicon wafer 10 by a thermal oxidation process;
[0036] For this step, the specific implementation is: after the hot oxygen equipment where the silicon wafer 10 is located is evacuated, oxygen is introduced until the normal pressure is restored, and the temperature is heated to 580°C to 640°C. For example, this step can be heated to 580°C, 590°C, 600°C, 605°C, 608°C, 610°C, 615°C, 620°C, 630°C or 640°C. The silicon wafer 10 is made to grow a tunneling oxide layer 20 in an oxygen atmosphere. The main component of the tunneling oxide layer 20 formed in this step is silicon dioxide (SiO2). The oxygen element in the oxygen enters the first main surface of the silicon wafer and forms SiO2 with the single crystal silicon Si on the first main surface.
[0037] The structural changes after this step are as follows Figure 2 and Figure 3 The direction from the top to the bottom of the quartz boat is as shown in Figure 3 Direction D as shown. Figure 3 As shown in FIG. 1 , the tunnel oxide layer 20 formed on the surface of the silicon wafer 10 in this step decreases along the direction D. This is because the uniformity of the high-temperature epitaxially grown tunnel oxide layer 20 is affected by the temperature field and the gas field. The heat of the silicon wafer 10 near the bottom of the quartz boat will be partially absorbed (e.g. Figure 3 The oxygen concentration in the area of the silicon wafer 10 located at the bottom of the quartz boat is also lower than that in the area located at the top of the quartz boat due to the obstruction of the quartz boat. Figure 3 The tunnel passivation effect of the thinner area of the tunnel oxide layer (such as the area near the edge of a) is shown. Figure 3 The area near the edge of b shown in the figure will be destroyed, the separation effect of the high and low junction electron-hole pairs will be weakened, and the passivation effect will be lost; if the thinnest area (such as Figure 3 The tunnel passivation effect of the region near the edge of b is shown in Figure 1. Although in theory the thicker region of the tunnel oxide layer (such as Figure 3 The passivation effect can be achieved in the region near the edge of a as shown, but it is not easy for majority carriers to pass through the thicker region, resulting in limited tunnel passivation and increased recombination of minority carriers near the tunnel oxide layer, resulting in a passivated contact solar cell being prepared.
[0038] In this step, a tunneling oxide layer is prepared on a silicon wafer as follows: Figure 3 In the direction D shown (from the top to the bottom of the quartz boat), the thickness of the tunnel oxide layer on the silicon wafer decreases, and the area of the tunnel oxide layer formed on the silicon wafer near the top of the quartz boat (i.e. Figure 3 The area near the edge of a shown in the figure) and the area near the bottom of the quartz boat (i.e. Figure 3 The thickness difference between the region near the edge b shown in the figure is 0.2nm to 0.8nm. For example, the thickness difference of the tunneling oxide layer formed on the silicon wafer is 0.2nm, 0.3nm, 0.4nm, 0.5nm, 0.6nm, 0.7nm, 0.8nm, etc. By adjusting the thickness difference of the tunneling oxide layer, a better match can be formed between the tunneling oxide layer and the barrier layer formed subsequently.
[0039] Step S103: controlling the wafer inserting machine to change the direction of the silicon wafer in the quartz boat;
[0040] Specifically, the upper and lower positions of the silicon wafers in the quartz boat are swapped. Figure 3As shown, the silicon wafer whose edge a was originally close to the top of the quartz boat and edge b was close to the bottom of the quartz boat is adjusted to have edge a close to the bottom of the quartz boat and edge b close to the top of the quartz boat by a wafer inserter, so that the barrier layer 40 formed subsequently can also be thinned along direction D, that is, the thickness of the barrier layer 40 decreases from edge b to edge a of the silicon wafer. In other words, the barrier layer 40 formed on the silicon wafer is thicker in the area closer to edge b, and thinner in the area closer to edge a. This is opposite to the decreasing direction of the thickness of the tunnel oxide layer 20 formed in step S102.
[0041] This step uses a boat insertion machine to adjust the silicon wafer, which is easy to operate and does not require the addition of other equipment, making the entire process simple.
[0042] Step S104: sequentially stacking a first intrinsic polysilicon layer 30 ′, a barrier layer 40 and a second intrinsic polysilicon layer 50 ′ on the tunnel oxide layer by chemical vapor deposition;
[0043] This step forms a stacked structure of a first intrinsic polysilicon layer 30', a barrier layer 40 and a second intrinsic polysilicon layer 50'. Figure 2 shown.
[0044] Specifically, the process of forming the first intrinsic polysilicon layer 30' in this step mainly includes: placing a quartz boat containing silicon wafers in a chemical vapor deposition device, and introducing silane gas at a temperature of 590°C to 620°C to grow the first intrinsic polysilicon layer 30' on the tunneling oxide layer. For example, the temperature of growing the first intrinsic polysilicon layer 30' can be controlled to be 590°C, 595°C, 600°C, 605°C, 608°C, 610°C, 615°C or 620°C, etc. Among them, in this step, the thickness of the first intrinsic polysilicon layer 30' formed is 20nm to 80nm. For example, the first intrinsic polysilicon layer 30' can be 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, etc.
[0045] Further, the process of stacking the barrier layer 4 on the first intrinsic polysilicon layer 30' in this step mainly includes: closing the silane gas, and after evacuating, introducing oxygen until normal pressure, and growing the barrier layer 40 on the first intrinsic polysilicon layer 30' at a temperature of 570°C to 610°C. For example, the barrier layer 40 can be grown at a temperature of 570°C, 580°C, 590°C, 600°C or 610°C. In other words, the barrier layer formed in this step is also SiO2. The thickness of the barrier layer formed in this step can be 2nm to 5nm. Among them, the difference between the thin area and the thick area of the barrier layer 40 formed in this step is 0.4 to 1.0nm. For example, the difference between the thin area and the thick area can be 0.4nm, 0.5nm, 0.6nm, 0.8nm, 1.0nm, etc. It is worth noting that the thickness of the barrier layer 40 is within the range of 2nm to 5nm, which generally means that the thickness of each position of the barrier layer is within the range of 2nm to 5nm. That is, the thickness of the thinnest position of the barrier layer 40 is not less than 2nm, and the thickness of the thickest position is not more than 5nm. For example, the thickness of any position of the barrier layer can be 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 5nm, etc. The thicker area of the barrier layer 40 mainly plays a blocking role, so that in the subsequent doping process of the doping element, after the doping element reaches the first intrinsic polysilicon layer 30', only a small amount of the doping element passes through the tunnel oxide layer to reach the first main surface of the silicon wafer to form N + -Si. The thinner area of the barrier layer 40 allows more doping elements to penetrate into the first intrinsic polysilicon layer 30'. More doping elements that penetrate into the first intrinsic polysilicon layer 30' can cause a pinhole effect in the thicker tunnel oxide layer, thereby ensuring that the majority carriers can pass through the tunnel oxide layer, reducing the recombination of minority carriers near the tunnel oxide layer 20, and effectively improving the contact and passivation performance.
[0046] Further, the process of stacking and forming the second intrinsic polysilicon layer 50' on the barrier layer 40 in this step mainly includes: turning off the oxygen, and after evacuation, re-introducing the silane gas, and growing the second intrinsic polysilicon layer 50' on the barrier layer 40 at a temperature of 590°C to 620°C. For example, the temperature of the second intrinsic polysilicon layer 50' can be controlled to be 590°C, 600°C, 608°C, 610°C, 615°C or 620°C. The thickness of the second intrinsic polysilicon layer can be 40 to 120nm. For example, the thickness of the second intrinsic polysilicon layer can be 40nm, 45nm, 50nm, 55nm, 60nm, 70nm, 75nm, 80nm, 90nm, 100nm, 110nm, 120nm, etc.
[0047] Through research, it is found that after the subsequent step S105 of thermal diffusion doping treatment, the barrier layer 4, in addition to its barrier function, will also undergo a phosphorus expulsion phenomenon, that is, phosphorus enrichment and increased phosphorus concentration will occur on both sides of the barrier layer 4. The embodiment of the present invention can avoid the influence of the phosphorus expulsion phenomenon on the tunneling oxide layer, the first doped polysilicon layer 30 and the second doped polysilicon layer 50 by designing the thickness of the first intrinsic polysilicon layer 30' to be 20nm to 80nm and the thickness of the second intrinsic polysilicon layer to be 40 to 120nm.
[0048] It is worth noting that during the process of forming the first intrinsic polysilicon layer 30' and the second intrinsic polysilicon layer 50' in the above steps, the thickness of the first intrinsic polysilicon layer 30' and the thickness of the second intrinsic polysilicon layer 50' at various locations on the silicon wafer can be substantially evenly distributed.
[0049] Step S105: Perform a doping element thermal diffusion activation process on the first intrinsic polysilicon layer 30' and the second intrinsic polysilicon layer 50' to form the first doped polysilicon layer 30 and the second doped polysilicon layer 50. The specific implementation of step S105 is: at a temperature of 800°C to 900°C, the first intrinsic polysilicon layer 30' and the second intrinsic polysilicon layer 50' are phosphorus diffused and activated by POCl3 and O2. For example, the phosphorus diffusion temperature can be 800°C, 820°C, 830°C, 850°C, 870°C, 880°C, 890°C or 900°C.
[0050] For N-type silicon wafers, the doping element used in this step is generally phosphorus, and for P-type silicon wafers, the doping element used in this step is generally boron. Preferably, for N-type silicon wafers, the doping element used in this step is phosphorus.
[0051] The doping concentration of the first doped polysilicon layer 30 and the second doped polysilicon layer 50 formed in step S105 are within 2E 20 atoms / cm 3 ~8E 20 atoms / cm 3 , and the doping concentration of the first doped polysilicon layer 30 is lower than the doping concentration of the second doped polysilicon layer 50. Further, the doping concentration of the first doped polysilicon layer 30 is 0.1 to 3E lower than the doping concentration of the second doped polysilicon layer 50. 20 atoms / cm 3 For example, the doping concentration of the first doped polysilicon layer 30 is 0.1 atoms / cm lower than the doping concentration of the second doped polysilicon layer 50. 3 、0.5atoms / cm 3 , 1atoms / cm 3 , 1E 5 atoms / cm3 , 1E 8 atoms / cm 3 , 1E 10 atoms / cm 3 , 2E 10 atoms / cm 3 , 5E 10 atoms / cm 3 , 2E 15 atoms / cm 3 , 3E 20 atoms / cm 3 Preferably, the difference between the doping concentration of the first doped polysilicon layer 30 and the doping concentration of the second doped polysilicon layer 50 is 1E 20 atoms / cm 3 .
[0052] Taking N-type silicon wafer as an example, through the above processing, a structure is formed on the first main surface of the silicon wafer: N-Si / N + -Si / SiO 2-1 / N1 ++ Poly-Si / SiO 2-2 / N2 ++ Poly-Si, where N-Si represents silicon wafer; N + -Si represents an intrinsically doped single crystal layer formed on the first main surface of the silicon wafer by the doping element; SiO 2-1 Indicates tunneling oxide layer; N1 ++ Poly-Si represents the first doped polysilicon layer 30; SiO 2-2 N2 represents the barrier layer 40; ++ Poly-Si represents the second doped polysilicon layer 50. + -Si is a doping element that passes through SiO 2-1 Formed by SiO 2-1 and SiO 2-2 In combination, the tunnel oxide layer can enhance the blocking effect of minority carriers and improve the tunnel passivation effect. 2-1 and SiO 2-2 Matching N + -Si and N ++ Appropriate high and low potential barriers are formed between Poly-Si to enhance the separation effect of high and low junction electron-hole pairs.
[0053] That is, the technical solution provided by the embodiment of the present invention is to first form the first intrinsic polysilicon layer 30' and the second intrinsic polysilicon layer 50', and then achieve synchronous doping of the first intrinsic polysilicon layer 30' and the second intrinsic polysilicon layer 50' through a one-step process to obtain the first doped polysilicon layer 30 and the second doped polysilicon layer 50. This effectively simplifies the processing process of the passivated contact solar cell and makes each process controllable.
[0054] exist Figure 1 In the preparation method provided, the arrangement order of the silicon wafers is adjusted after the tunnel oxide layer is prepared, and then a first intrinsic polysilicon layer, a barrier layer and a second intrinsic polysilicon layer are sequentially stacked on the adjusted silicon wafer, so that a thicker barrier layer is formed in a thinner area of the tunnel oxide layer on the silicon wafer, and a thinner barrier layer is formed on a thicker area with the tunnel oxide layer, that is, by matching the thickness of the tunnel oxide layer with the thickness of the barrier layer, the thicker area of the tunnel oxide layer is matched with the thinner barrier layer, so that the ability of the barrier layer to block doped elements is reduced, so that the tunnel oxide layer can produce a sufficient pinhole effect, and the thinner area of the tunnel oxide layer is matched with the thicker barrier layer, so that the ability to block the diffusion of doped elements is improved, and the doped elements are prevented from destroying the tunnel oxide layer, thereby improving the preparation process of the passivation contact solar cell and effectively improving the yield of the passivation contact solar cell with excellent passivation contact performance.
[0055] Furthermore, due to the cooperation between the tunnel oxide layer and the barrier layer, the above steps can be completed within a wider process window. In particular, the process window for diffusion of doping elements is significantly increased, and inefficient wafers caused by unstable doping element diffusion process and uneven temperature zones are reduced. While improving the yield, the process difficulty and precision can be effectively reduced, mass production can be achieved, and it is conducive to industrial promotion.
[0056] In addition, the entire preparation process can be completed using existing solar cell preparation equipment without adding other equipment, which can effectively control production costs.
[0057] Furthermore, after the above step S105, it may further include: forming a back passivation layer 90 on the second doped polysilicon layer 50. The thickness of the back passivation layer 90 may be 75 to 85 nm. For example, the thickness of the back passivation layer 90 may be 75 nm, 76 nm, 78 nm, 79 nm, 80 nm, 81 nm, 82 nm, 83 nm, 84 nm, 85 nm, etc. The passivation contact effect achieved by the cooperation between the tunneling oxide layer 20, the first doped polysilicon layer 30, the barrier layer 40 and the second doped polysilicon layer 50 may be further enhanced by setting the thickness of the passivation layer 90.
[0058] Furthermore, by matching the thickness of the tunneling oxide layer with the thickness of the barrier layer, the tunneling oxide layer can be further thinned, ensuring that when the passivation is normal, the contact resistivity caused by the tunneling oxide layer can be reduced and the fill factor can be increased.
[0059] Furthermore, before the above step S101, the following steps may be further included: step 01 and step 02.
[0060] Specifically, step 01: forming a PN junction emitter 60 and a doped silicon glass layer by in-situ diffusion on the second main surface of the double-textured silicon wafer, wherein the doping element type contained in the PN junction emitter 60 is opposite to the doping element type contained in the first doped polysilicon layer;
[0061] The emitter 60 of the PN junction is obtained by directly diffusing doping elements on the second main surface of the silicon wafer.
[0062] For example, if the doping element type included in the first doped polysilicon layer is N-type, then the doping element type included in the emitter 60 of the PN junction is P-type, that is, a P+ emitter; if the doping element type included in the first doped polysilicon layer is P-type, then the doping element type included in the emitter 60 of the PN junction is N-type, that is, an N+ emitter. Preferably, the emitter 60 of the PN junction is a P+ emitter.
[0063] Step 02: clean the emitter 60 of the PN junction and the doped silicon glass layer plated on the first main surface of the silicon wafer, and polish the first main surface of the silicon wafer.
[0064] The polishing process can ensure that the emitter 60 of the PN junction formed on the first main surface of the silicon wafer and the doped silicon glass layer are cleaned.
[0065] The processing of step 01 and step 02 can be completed by using existing processing technology, which will not be described in detail here.
[0066] Furthermore, the above preparation method further includes: growing an aluminum oxide film layer 70 on the second main surface of the silicon wafer by atomic layer deposition (ALD).
[0067] In addition, the above preparation method further comprises: growing a front passivation layer 80 on the second main surface of the silicon wafer by plasma enhanced chemical vapor deposition (PECVD).
[0068] Another embodiment of the present invention provides a method for preparing a passivated contact solar cell. Figure 4 As shown, the preparation method may include the following steps:
[0069] Step S401: Arrange and place the silicon wafers with double textured structure in a quartz boat.
[0070] Step S402: forming a PN junction emitter and a doped silicon glass layer by in-situ diffusion on the second main surface of the double textured silicon wafer, wherein the PN junction emitter contains doping elements of a type opposite to that of the first doped polysilicon layer.
[0071] Step S403: cleaning the emitter of the PN junction and the doped silicon glass layer plated on the first main surface of the silicon wafer, and polishing the first main surface of the silicon wafer.
[0072] Step S404: After the hot oxygen equipment where the silicon wafer is located is evacuated, oxygen is introduced until the pressure returns to normal, and the temperature is heated to 580° C. to 640° C., so that the silicon wafer grows a tunnel oxide layer in the oxygen atmosphere.
[0073] Step S405: controlling the wafer inserting machine to adjust the up and down directions of the silicon wafer on the quartz boat.
[0074] Step S406: placing the quartz boat containing the silicon wafers in a chemical vapor deposition device, and introducing silane gas at a temperature of 590° C. to 620° C. to grow a first intrinsic polysilicon layer on the tunneling oxide layer.
[0075] Step S407: Turn off the silane gas, evacuate the air, introduce oxygen until the pressure reaches normal, and grow a barrier layer on the first intrinsic polysilicon layer at a temperature of 570° C. to 610° C.
[0076] Step S408: turn off the oxygen, evacuate the air, and then reintroduce silane gas to grow a second intrinsic polysilicon layer on the barrier layer at a temperature of 590° C. to 620° C.
[0077] Step S409: at a temperature of 800° C. to 900° C., phosphorus is diffused and activated on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer by using POCl 3 and O 2 .
[0078] Step S410: growing an aluminum oxide film layer on the second main surface of the silicon wafer by ALD.
[0079] Step S411: growing a passivation layer on the second doped polysilicon layer and the aluminum oxide film layer by PECVD.
[0080] Step S412: Printing metal electrodes on the front and back sides of the silicon wafer respectively by screen printing.
[0081] Through the above Figure 4 The structure of the passivated contact solar cell obtained by the process of the embodiment shown is as follows Figure 5 shown.
[0082] Furthermore, an embodiment of the present invention provides a passivated contact solar cell. Figure 5 As shown, the passivated contact solar cell may include: a silicon wafer 10, a tunneling oxide layer 20 stacked on a first main surface of the silicon wafer 10, a first doped polysilicon layer 30, a barrier layer 40, and a second doped polysilicon layer 50, wherein:
[0083] The thickness of the tunnel oxide layer 20 decreases along the first direction, and the thickness of the barrier layer 40 decreases along the second direction, wherein the first direction is completely opposite to the second direction. Figure 3 As shown, the first direction is the direction consistent with direction D, and the second direction is the direction opposite to direction D. The first direction generally refers to the direction from edge a located at the top of the quartz boat to edge b located at the bottom of the quartz boat when the silicon wafer is inserted into the quartz boat during the preparation of the tunnel oxide layer. Correspondingly, the second direction is the direction from edge b to edge a of the silicon wafer. Both the first direction and the second direction are parallel to the side of the silicon wafer that is perpendicular to edges a and b.
[0084] The doping element type included in the first doped polysilicon layer 30 is consistent with the doping element type included in the second doped polysilicon layer 50; for example, for an N-type silicon wafer, the doping element type is N-type, and for a P-type silicon wafer, the doping element type is P-type.
[0085] The doping concentration of the first doped polysilicon layer 30 is lower than the doping concentration of the second doped polysilicon layer 50. The doping concentration of the first doped polysilicon layer 30 and the doping concentration of the second doped polysilicon layer 50 are generally within a range of 2E. 20 atoms / cm 3 ~8E 20 atoms / cm 3 The doping concentration of the first doped polysilicon layer 30 is lower than the doping concentration of the second doped polysilicon layer 50. Further, the doping concentration of the first doped polysilicon layer 30 is 0.1 to 3E lower than the doping concentration of the second doped polysilicon layer 50. 20 atoms / cm 3 For example, the doping concentration of the first doped polysilicon layer 30 is 0.1 atoms / cm lower than the doping concentration of the second doped polysilicon layer 50. 3 、0.5atoms / cm 3 , 1atoms / cm 3 , 1E 5 atoms / cm 3 , 1E 8 atoms / cm 3 , 1E 10 atoms / cm 3 , 2E 10atoms / cm 3 , 5E 10 atoms / cm 3 , 2E 15 atoms / cm 3 , 3E 20 atoms / cm 3 Preferably, the difference between the doping concentration of the first doped polysilicon layer 30 and the doping concentration of the second doped polysilicon layer 50 is 1E 20 atoms / cm 3 .
[0086] The passivated contact solar cell is obtained based on the preparation method of the passivated contact solar cell provided in the above embodiment.
[0087] The thickness of the first doped polysilicon layer 30 is 20 nm to 80 nm; for example, the first doped polysilicon layer 30 may be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, etc.
[0088] In addition, the thickness of the barrier layer 40 may be 2nm to 5nm. It is worth noting that the thickness of the barrier layer 40 is within the range of 2nm to 5nm, which generally means that the thickness of each position of the barrier layer is within the range of 2nm to 5nm. That is, the thickness of the barrier layer 40 at the thinnest position is not less than 2nm, and the thickness at the thickest position is not more than 5nm. For example, the thickness of any position of the barrier layer may be 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 5nm, etc.
[0089] Furthermore, the thickness of the second doped polysilicon layer 50 is 40 to 120 nm; for example, the thickness of the second intrinsic polysilicon layer may be 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 70 nm, 75 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, etc.
[0090] Furthermore, if Figure 5 As shown, the passivated contact solar cell may further include:
[0091] The emitter 60 of the PN junction is arranged on the second main surface of the silicon wafer 10, wherein the doping element type contained in the emitter 60 of the PN junction is opposite to the doping element type contained in the first doped polysilicon layer 30. For example, if the doping element type of the first doped polysilicon layer 30 is N-type, the doping element type contained in the emitter 60 of the PN junction is P-type, that is, the emitter 60 of the PN junction is a P+ emitter; if the doping element type of the first doped polysilicon layer 30 is P-type, the doping element type contained in the emitter 60 of the PN junction is N-type, that is, the emitter 60 of the PN junction is an N+ emitter. Preferably, the emitter 60 of the PN junction is a P+ emitter.
[0092] Furthermore, if Figure 5 As shown, the passivated contact solar cell may also include: an aluminum oxide film layer 70 and a front passivation layer 80 stacked on the emitter 60 of the PN junction, a back passivation layer 90 stacked on the second doped polysilicon layer 50, and metal electrodes 100 respectively arranged on the front and back of the silicon wafer.
[0093] The above-mentioned passivation contact solar cell controls the thickness of the tunneling oxide layer 20 and the thickness of the barrier layer 40 to decrease in opposite directions, so that a thinner tunneling oxide layer 20 is matched with a thicker barrier layer 40, and a thicker tunneling oxide layer 20 is matched with a thinner barrier layer 40, thereby improving the passivation contact performance of excellent passivation contact solar cells and the yield rate of passivation contact solar cells with excellent passivation contact performance.
[0094] Example:
[0095] S1: Double-sided texturing is performed on an N-type single-crystalline silicon wafer with a resistivity of 0.9Ωcm and a thickness of 130μm. The silicon wafer is then loaded into a quartz boat using a boat inserter, and boron is diffused on the light-receiving side of the single-crystalline silicon wafer to form a boron-doped layer and a borosilicate glass layer. The borosilicate glass layer coated on the backlight side of the single-crystalline silicon wafer is removed by HF, and polished with an alkaline solution to form a back-light polished silicon wafer with a tower base morphology of 8 to 10μm on the back.
[0096] S2: placing the quartz boat loaded with the silicon wafer processed in step S1 in a thermal oxygen process treatment device, evacuating the vacuum, introducing 10000 sccm of oxygen until returning to normal pressure, and heating to 605° C. to grow a tunneling oxide layer of about 1.5 nm in an oxygen atmosphere.
[0097] S3: The silicon wafers processed in step S2 loaded on the quartz boat are swapped up and down by using a boat inserting machine, that is, the one at the bottom is adjusted to the top.
[0098] S4: The silicon wafer after the position change in step S3 is sent to the CVD equipment, silane is introduced at 608°C to grow a first intrinsic polysilicon layer with a thickness of 50nm, the silane is turned off, and after vacuuming, oxygen is introduced to restore the pressure to normal pressure, and a barrier layer (SiO2 layer) of about 2.5nm is grown at 600°C. Subsequently, the oxygen is turned off, and after vacuuming, silane is introduced to grow a second intrinsic polysilicon layer with a thickness of 70nm at a temperature of 605°C.
[0099] Step S5: Adjust the CVD equipment to 890°C, introduce POCl3 and O2, complete phosphorus diffusion on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer, and anneal for activation. Back side structure of silicon wafer: N-Si / N + -Si / SiO 2-1 / N1 ++ Poly-Si / SiO2-2 / N2 ++ Poly-Si.
[0100] Step S6: Cleaning the borosilicate glass layer (BSG) coated on the front side of the silicon wafer and the phosphosilicate glass layer (PSG) on the back side.
[0101] Step S7: ALD is used to coat the front velvet surface of the silicon wafer to grow 4.5 nm of Al2O3.
[0102] Step S8: Use PECVD equipment to grow a passivation layer (SiN) of about 72 nm on the front side of the silicon wafer. x Thin film), a passivation layer (SiN x film).
[0103] Step S9: Use screen printing to print silver paste on the front and back sides of the silicon wafer, respectively, and the width of the front and back fine grids is about 14 μm. Finally, after sintering and light injection treatment, an N-type Topcon cell is obtained.
[0104] By using the fact that the thick or thin areas of the two oxide layers are not on the lower or upper surface at the same time, phosphorus diffusion is more uniform, the phosphorus source entering the Si substrate is evenly distributed, the tailing state of the ECV curves tested in different areas is similar, the uneven brightness of PL is reduced, and the yield rate of the battery is significantly increased. The back structure of the silicon wafer is, where N1 ++ Poly-Si and N2 ++ The doping concentration of Poly-Si is 5E 20 atoms / cm 3 , and N1 ++ The doping concentration in Poly-Si is higher than that in N2 ++ The doping concentration of Poly-Si is about 1E lower 20 atoms / cm 3 .
[0105] Comparative Example:
[0106] Compared with the above embodiment, this comparative example lacks step S3. Step S4 adopts LPCVD (Low Pressure Chemical Vapor Deposition) to directly grow an intrinsic polysilicon layer. The thickness of the intrinsic polysilicon layer grown in this step is 120nm (that is, the thickness of the intrinsic polysilicon layer grown in this step is the sum of the thickness of the first intrinsic polysilicon layer and the second intrinsic polysilicon layer of the above embodiment), and other steps are the same as those of the above embodiment.
[0107] The solar cells obtained in the above embodiment and the comparative example were subjected to performance tests, and the test results are shown in Table 1. As can be seen from Table 1, compared with the comparative example, the current density (Jsc (mA / cm 2 )) is 41.51mA / cm 2 , the open circuit voltage (Voc(V)) is 0.7365V, the fill factor (FF%) is 85.60%, and the cell efficiency (Eta(%)) is 26.17%. Compared with the comparative example, the open circuit voltage (Voc(V)) of the passivated contact solar cell prepared by the preparation method provided in the embodiment of the present invention is increased by 0.0013V (i.e. 1.3mV), the fill factor (FF%) is increased by about 0.1%, and the cell efficiency (Eta(%)) is also increased by about 0.1%.
[0108] Table 1
[0109] project <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) Eta(%) Comparative Example 41.49 0.7352 85.51 26.08 Example 41.51 0.7365 85.60 26.17
[0110] It is worth noting that the test results of the comparative example and the test results of the embodiment in Table 1 are obtained in the following manner: batches of passivated contact solar cells with different structures are prepared by the embodiment and the comparative example, and the batches of passivated contact solar cells with different structures are tested. After discarding the passivated contact solar cells with abnormally increased or decreased test results, the current density (Jsc (mA / cm 2 )), open circuit voltage (Voc(V)), fill factor and battery efficiency (Eta(%)).
[0111] In summary, the embodiments of the present invention provide the following technical solutions:
[0112] Technical solution 1, a method for preparing a passivated contact solar cell, comprising:
[0113] Step 1, placing the silicon wafer in a quartz boat;
[0114] Step 2: preparing a tunneling oxide layer on the first main surface of the silicon wafer by a thermal oxidation process;
[0115] Step 3, controlling the wafer inserting machine to change the direction of the silicon wafer in the quartz boat;
[0116] Step 4, sequentially stacking a first intrinsic polysilicon layer, a barrier layer, and a second intrinsic polysilicon layer on the tunnel oxide layer by chemical vapor deposition;
[0117] Step 5: Perform a doping element thermal diffusion activation process on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer to form a first doped polysilicon layer and a second doped polysilicon layer.
[0118] Technical solution 2: According to the method for preparing a passivated contact solar cell according to technical solution 1, step 2 comprises:
[0119] After the hot oxygen equipment where the silicon wafer is located is evacuated, oxygen is introduced until the normal pressure is restored, and the temperature is heated to 580° C. to 640° C., so that the silicon wafer grows a tunnel oxide layer in the oxygen atmosphere.
[0120] Technical solution 3: A method for preparing a passivated contact solar cell according to technical solution 1,
[0121] In step 2, the tunneling oxide layer prepared on the silicon wafer has a decreasing thickness, and the thickness difference between the area of the tunneling oxide layer formed on the silicon wafer close to the top of the quartz boat and the area close to the bottom of the quartz boat is between 0.2 and 0.8 nm.
[0122] Technical solution 4: According to the method for preparing a passivated contact solar cell according to technical solution 1, step 3 comprises:
[0123] The upper and lower positions of the silicon wafers in the quartz boat are exchanged.
[0124] Technical solution 5, according to the method for preparing a passivated contact solar cell according to technical solution 1, step 4 comprises:
[0125] Step 41, placing the quartz boat containing the silicon wafer in a chemical vapor deposition device, and introducing silane gas at a temperature of 590° C. to 620° C. to grow a first intrinsic polysilicon layer on the tunnel oxide layer;
[0126] Step 42, closing the silane gas, evacuating the gas, introducing oxygen until the pressure reaches normal, and growing a barrier layer on the first intrinsic polysilicon layer at a temperature of 570° C. to 610° C.;
[0127] Step 43, turning off the oxygen, evacuating the air, and then reintroducing silane gas to grow a second intrinsic polysilicon layer on the barrier layer at a temperature of 590° C. to 620° C.
[0128] Technical solution 6: A method for preparing a passivated contact solar cell according to technical solution 1 or 5,
[0129] The thickness of the first intrinsic polysilicon layer is 20nm to 80nm;
[0130] and / or,
[0131] The thickness of the barrier layer is 2nm to 5nm;
[0132] and / or,
[0133] The thickness of the second intrinsic polysilicon layer is 40-120 nm.
[0134] Technical solution 7: According to the method for preparing a passivated contact solar cell according to any one of technical solutions 1 to 5, step 5 comprises:
[0135] At a temperature of 800° C. to 900° C., phosphorus is diffused and activated on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer by using POCl 3 and O 2 .
[0136] Technical solution 8: A method for preparing a passivated contact solar cell according to any one of technical solutions 1 to 5,
[0137] The doping concentration of the first doped polysilicon layer and the doping concentration of the second doped polysilicon layer formed in step 5 are within 2E 20 atoms / cm 3 ~8E 20 atoms / cm 3 , and the doping concentration of the first doped polysilicon layer is lower than the doping concentration of the second doped polysilicon layer.
[0138] Technical solution 9: A method for preparing a passivated contact solar cell according to technical solution 8,
[0139] The doping concentration of the first doped polysilicon layer is 0.1 to 3E lower than the doping concentration of the second doped polysilicon layer. 20 atoms / cm 3 .
[0140] Technical solution 10: The method for preparing a passivated contact solar cell according to any one of technical solutions 1 to 5 and 9, further comprising:
[0141] Step 6: Form a passivation layer on the second doped polysilicon layer.
[0142] Technical solution 11, a method for preparing a passivated contact solar cell according to technical solution 10,
[0143] The thickness of the passivation layer is 75-85 nm.
[0144] Technical solution 12: The method for preparing a passivated contact solar cell according to technical solution 1, further comprising:
[0145] Step 01, forming an emitter of a PN junction and a doped silicon glass layer by in-situ diffusion on the second main surface of a silicon wafer with a double textured structure, wherein the type of doping elements contained in the emitter of the PN junction is opposite to the type of doping elements contained in the first doped polysilicon layer;
[0146] Step 02: clean the emitter of the PN junction and the doped silicon glass layer plated around the first main surface of the silicon wafer, and polish the first main surface of the silicon wafer.
[0147] Technical solution 13. The method for preparing a passivated contact solar cell according to technical solution 12 further includes:
[0148] Step 6', growing an aluminum oxide film layer on the second main surface of the silicon wafer by ALD;
[0149] Preferably, the passivation layer is grown on the second main surface of the silicon wafer by PECVD.
[0150] Technical solution 14, a passivated contact solar cell, comprising: a silicon wafer 10, a tunneling oxide layer 20 stacked on a first main surface of the silicon wafer 10, a first doped polysilicon layer 30, a barrier layer 40 and a second doped polysilicon layer 50, wherein:
[0151] The thickness of the tunnel oxide layer 20 decreases along a first direction, and the thickness of the barrier layer 40 decreases along a second direction, wherein the first direction is completely opposite to the second direction;
[0152] The type of doping element included in the first doped polysilicon layer 30 is consistent with the type of doping element included in the second doped polysilicon layer 50;
[0153] The doping concentration of the first doped polysilicon layer 30 is lower than the doping concentration of the second doped polysilicon layer 50 .
[0154] Technical solution 15. The passivated contact solar cell according to technical solution 14 further includes:
[0155] An emitter 60 of a PN junction is disposed on the second main surface of the silicon wafer 10 , wherein the type of doping elements included in the emitter 60 of the PN junction is opposite to the type of doping elements included in the first doped polysilicon layer 30 .
[0156] Technical solution 16. A passivated contact solar cell according to technical solution 14,
[0157] The thickness of the first doped polysilicon layer is 20nm to 80nm;
[0158] and / or,
[0159] The thickness of the barrier layer is 2nm to 5nm;
[0160] and / or,
[0161] The thickness of the second doped polysilicon layer is 40 to 120 nm;
[0162] and / or,
[0163] The doping concentration of the first doped polysilicon layer and the doping concentration of the second doped polysilicon layer are 2E 20 atoms / cm 3 ~8E 20 atoms / cm 3 , and the doping concentration of the first doped polysilicon layer is lower than the doping concentration of the second doped polysilicon layer;
[0164] Preferably, the doping concentration of the first doped polysilicon layer is 0.1 to 3E lower than the doping concentration of the second doped polysilicon layer. 20 atoms / cm 3 .
[0165] The introduction provided in the above steps is only used to help understand the method, structure and core idea of the present invention. For ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also belong to the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a passivated contact solar cell, It is characterized in that include: Step 1, placing the silicon wafer in a quartz boat; Step 2: preparing a tunneling oxide layer on the first main surface of the silicon wafer by a thermal oxidation process; Step 3, controlling the wafer inserting machine to change the direction of the silicon wafer in the quartz boat; Step 4, sequentially stacking a first intrinsic polysilicon layer, a barrier layer, and a second intrinsic polysilicon layer on the tunnel oxide layer by chemical vapor deposition; Step 5: Perform a doping element thermal diffusion activation process on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer to form a first doped polysilicon layer and a second doped polysilicon layer.
2. The method for preparing a passivated contact solar cell according to claim 1, It is characterized in that Step 2 includes: After the hot oxygen equipment where the silicon wafer is located is evacuated, oxygen is introduced until the normal pressure is restored, and the temperature is heated to 580° C. to 640° C., so that the silicon wafer grows a tunnel oxide layer in the oxygen atmosphere.
3. The method for preparing a passivated contact solar cell according to claim 1, It is characterized in that In step 2, the tunneling oxide layer prepared on the silicon wafer has a decreasing thickness, and the thickness difference between the area of the tunneling oxide layer formed on the silicon wafer close to the top of the quartz boat and the area close to the bottom of the quartz boat is between 0.2 and 0.8 nm.
4. The method for preparing a passivated contact solar cell according to claim 1, It is characterized in that Step 3 includes: The upper and lower positions of the silicon wafers in the quartz boat are exchanged.
5. The method for preparing a passivated contact solar cell according to claim 1, It is characterized in that Step 4 includes: Step 41, placing the quartz boat containing the silicon wafer in a chemical vapor deposition device, and introducing silane gas at a temperature of 590° C. to 620° C. to grow a first intrinsic polysilicon layer on the tunnel oxide layer; Step 42, closing the silane gas, evacuating the gas, introducing oxygen until the pressure reaches normal, and growing a barrier layer on the first intrinsic polysilicon layer at a temperature of 570° C. to 610° C.; Step 43, turning off the oxygen, evacuating the air, and then reintroducing silane gas to grow a second intrinsic polysilicon layer on the barrier layer at a temperature of 590° C. to 620° C.
6. The method for preparing a passivated contact solar cell according to claim 1 or 5, It is characterized in that The thickness of the first intrinsic polysilicon layer is 20nm to 80nm; and / or, The thickness of the barrier layer is 2nm to 5nm; and / or, The thickness of the second intrinsic polysilicon layer is 40-120 nm.
7. The method for preparing a passivated contact solar cell according to any one of claims 1 to 5, It is characterized in that Step 5 includes: At a temperature of 800℃~900℃, through POCl 3 and O 2 , phosphorus is diffused and activated on the first intrinsic polysilicon layer and the second intrinsic polysilicon layer.
8. The method for preparing a passivated contact solar cell according to any one of claims 1 to 5, It is characterized in that The doping concentration of the first doped polysilicon layer and the doping concentration of the second doped polysilicon layer formed in step 5 are within 2E 20 atoms / cm 3 ~8E 20 atoms / cm 3 , and the doping concentration of the first doped polysilicon layer is lower than the doping concentration of the second doped polysilicon layer.
9. The method for preparing a passivated contact solar cell according to claim 8, It is characterized in that The doping concentration of the first doped polysilicon layer is 0.1 to 3E lower than the doping concentration of the second doped polysilicon layer. 20 atoms / cm 3 .
10. A passivated contact solar cell, It is characterized in that include: A silicon wafer (10), a tunneling oxide layer (20), a first doped polysilicon layer (30), a barrier layer (40) and a second doped polysilicon layer (50) stacked on a first main surface of the silicon wafer (10), wherein: The thickness of the tunnel oxide layer (20) decreases along a first direction, and the thickness of the barrier layer (40) decreases along a second direction, wherein the first direction is completely opposite to the second direction; The type of doping element contained in the first doped polysilicon layer (30) is consistent with the type of doping element contained in the second doped polysilicon layer (50); The doping concentration of the first doped polysilicon layer (30) is lower than the doping concentration of the second doped polysilicon layer (50).