Secondary battery containing lithium-carbon material and preparation method thereof
By using a lithium carbon material layer formed of linear and/or tubular carbon materials in lithium secondary batteries, the problems of uneven deposition of metallic lithium anode and poor conductivity of the passivation layer are solved, and excellent cycle performance of lithium secondary batteries is achieved. and high energy density.
Patent Information
- Application Number
- CN202310401899.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
The uneven deposition of metallic lithium anode during the charge and discharge process leads to the growth of lithium dendrites, which poses risks of thermal runaway, fire and explosion. The poor conductivity of the passivation layer leads to poor cycle performance, limiting its application in lithium secondary batteries.
A lithium carbon material layer formed of linear and/or tubular carbon materials is evenly distributed on the surface of the lithium-containing core to form a cocoon structure, which improves conductivity and inhibits the growth of lithium dendrites, improving cycle performance.
It achieves uniform current density, alleviates the volume expansion of the negative electrode, significantly improves the cycle performance and energy density of lithium secondary batteries, and provides new ideas for the industrialization of powdered lithium-containing materials.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a secondary battery containing lithium-carbon material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are the most widely used secondary batteries. However, due to the limited specific capacity of the embedded positive and negative electrode materials, their energy density has gradually approached the theoretical limit and is difficult to meet the growing market demand. The metallic lithium negative electrode has an extremely high specific capacity (3860mAh g -1 ), the lowest redox potential (-3.04Vvs.SHE (Standard hydrogen electrode)) and can be used with LiCoO2, LiNi x Co y Mn z The advantages of building battery systems with different positive electrode materials such as O2, S or O2 have once again become the focus of research.
[0003] However, the uneven deposition of lithium metal in the lithium metal anode during the charge and discharge process leads to the uncontrollable growth of lithium dendrites, which not only poses serious safety hazards such as thermal runaway, fire, and even explosion of the working battery, but also the freshly exposed lithium will continuously consume the electrolyte, resulting in poor cycle stability, which seriously hinders the practical application of lithium metal anode in rechargeable batteries. Therefore, researchers design or improve the morphology of lithium metal to solve the above problems.
[0004] Metal lithium powder is a granular metal lithium with very high activity and strict requirements on the use environment. CN 101213039 B discloses a method for stabilizing metal lithium powder. The method comprises the following steps: heating the metal lithium to a temperature exceeding its melting point, stirring the molten metal lithium and contacting the metal lithium with a fluorinating agent to provide stabilized metal lithium powder. The surface of the stabilized lithium powder forms dense and smooth lithium fluoride, but the lithium fluoride has poor conductivity, which will lead to uneven consumption of the negative electrode in practical applications, resulting in incomplete utilization of the capacity of the metal lithium powder and poor cycle performance, limiting its application.
[0005] How to develop a lithium secondary battery using powdered lithium-containing materials as raw materials while overcoming the problem of incomplete capacity due to poor conductivity of the metal lithium powder passivation layer and the poor cycle performance of metal lithium has become an urgent problem to be solved at this stage. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a secondary battery containing lithium-carbon material and a preparation method thereof, wherein the negative electrode of the secondary battery has a lithium-carbon material layer on the surface of the current collector, and the lithium-carbon material in the lithium-carbon material layer includes a cocoon formed by linear and / or tubular carbon materials and one or more lithium-containing cores contained in the cocoon. The carbon material in the lithium-carbon material layer is evenly distributed between the lithium-containing cores, which solves the problem of poor conductivity of the passivation layer, makes the current density uniform, and inhibits the growth of lithium dendrites. The secondary battery uses powdered lithium-containing materials as raw materials and has excellent cycle performance.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In the first aspect, the present invention provides a secondary battery containing lithium-carbon material, wherein the secondary battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a current collector and a lithium-carbon material layer arranged on the surface of the current collector, and the lithium-carbon material in the lithium-carbon material layer is composed of a cocoon formed by linear and / or tubular carbon material and one or more lithium-containing cores contained in the cocoon.
[0009] In the present invention, the good conductivity and toughness of the carbon material are utilized to wrap around the surface of the lithium-containing core to form a powdered lithium-containing active substance. In the process of preparing the negative electrode, the carbon material is evenly distributed between or inside the lithium-containing cores, thereby solving the problem of poor conductivity of the passivation layer on the surface of the lithium-containing core, making the current density uniform, inhibiting the growth of lithium dendrites, and alleviating the volume expansion of the negative electrode. It has excellent cycle performance and provides new ideas for the industrialization of lithium-containing materials such as powdered lithium-carbon materials.
[0010] In the present invention, there is no specific requirement for the shape and size of the secondary battery, which may be a square stacked type, a cylindrical stacked type, a cylindrical wound type, a square wound type, etc., or a new shape such as a hexagonal shape.
[0011] Optionally, the cocoon may contain one lithium-containing core, or may contain multiple lithium-containing cores, such as 2-5 lithium-containing cores. Preferably, a single cocoon contains one lithium-containing core.
[0012] Optionally, the average particle size of the lithium-containing core is 1-100 microns, for example, it can be 1 micron, 3 microns, 5 microns, 10 microns, 20 microns, 25 microns, 30 microns, 40 microns, 50 microns, 60 microns, 70 microns, 80 microns, 90 microns or 100 microns, including but not limited to the listed values, preferably 1-30 microns.
[0013] Optionally, the average particle size of the cocoon body is 1-100 microns, for example, it can be 1 micron, 2 microns, 5 microns, 10 microns, 20 microns, 25 microns, 30 microns, 40 microns, 50 microns, 60 microns, 70 microns, 80 microns, 90 microns or 100 microns, etc., including but not limited to the listed values, preferably 5-30 microns; the average thickness is 0.05-2 microns, for example, it can be 0.01 micron, 0.02 micron, 0.05 micron, 0.1 micron, 0.15 micron, 0.3 micron, 0.5 micron, 1 micron, 1.5 microns or 2 microns, etc., including but not limited to the listed values.
[0014] Optionally, the cocoon body has through holes with an average pore size of 10 to 50 nm, and the average pore size may be 10 nm, 12 nm, 15 nm, 20 nm, 30 nm, 40 nm, 45 nm or 50 nm, etc., including but not limited to the listed values.
[0015] Optionally, the lithium-containing core includes metallic lithium powder and / or metallic lithium alloy powder, preferably metallic lithium alloy powder. The metallic lithium alloy powder can effectively avoid the growth of lithium dendrites and has higher safety.
[0016] Optionally, the lithium alloy powder includes but is not limited to binary alloys and / or ternary alloys, the binary alloy powder includes but is not limited to any one of lithium boron alloy, lithium silver alloy, lithium indium alloy, lithium silicon alloy, lithium aluminum alloy or lithium tin alloy, or a combination of at least two of them; the ternary alloy powder includes but is not limited to any one of lithium tin silver alloy, lithium silver silicon alloy or lithium boron zinc alloy, or a combination of at least two of them.
[0017] Optionally, the current collector includes any one of copper foil, foam copper, PET composite copper foil, perforated copper foil, nickel foil, foam nickel, perforated nickel foil, carbon nanotube paper or graphene paper, or a combination of at least two of them, preferably any one of perforated copper foil, perforated nickel foil, carbon nanotube paper or graphene paper, or a combination of at least two of them. The preferred current collector has a small density and a high energy density of the secondary battery, which meets market demand.
[0018] Optionally, the ratio of the thickness of the lithium-carbon material layer to the current collector is (1-100):1, for example, it can be 1:1, 2:1, 5:1, 8:1, 10:1, 12:1, 15:1, 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1 or 100:1, but is not limited to the listed values. Within the thickness ratio range, the lithium secondary battery has a higher energy density and excellent cycle performance, preferably (5-80):1.
[0019] Optionally, the linear and / or tubular carbon material in the negative electrode includes any one or a combination of at least two of single-walled carbon nanotubes, few-walled carbon nanotubes, multi-walled carbon nanotubes, doped carbon nanotubes, carbon nanofibers or doped carbon nanofibers.
[0020] Optionally, the doping element in the doped carbon nanotubes and / or doped carbon nanofibers includes any one of nitrogen, oxygen, silver, silicon, tin or zinc, or a combination of at least two of them.
[0021] Optionally, the mass ratio of the linear and / or tubular carbon material to the lithium-containing core in the negative electrode is 1:
[0022] (50-1000), for example, it can be 1:50, 1:80, 1:100, 1:120, 1:150, 1:200, 1:300, 1:400, 1:450, 1:500, 1:700, 1:900 or 1:1000, etc., but is not limited to the listed values. Within the mass ratio range, the lithium secondary battery has higher conductivity and energy density, preferably 1:
[0023] (100-500).
[0024] In the present invention, the preparation method of the lithium-carbon material is not limited, as long as a cocoon formed by a linear and / or tubular carbon material and a lithium-carbon material containing one or more lithium-containing cores in the cocoon can be obtained, the lithium-carbon material is applicable to the present invention. For example, the lithium-carbon material can be prepared by the following method:
[0025] Metal lithium powder or lithium alloy powder is uniformly mixed with linear and / or tubular carbon material (such as single-walled carbon nanotubes) in a solvent (such as n-hexane), and then spray-dried or stirred at high speed to obtain a cocoon formed by the linear and / or tubular carbon material and a lithium-carbon material containing one or more metal lithium powder or lithium alloy powder particles in the cocoon.
[0026] Optionally, the N / P ratio of the secondary battery is 2 to 6, for example, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6, preferably 3-5, where the N / P ratio refers to the ratio of the negative electrode capacity to the positive electrode capacity of the battery.
[0027] Optionally, the positive electrode active material includes any one of elemental sulfur, oxygen, lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, or a combination of at least two thereof, preferably lithium iron phosphate (LFP) and / or lithium nickel cobalt manganese oxide (NCM).
[0028] Optionally, the electrolyte includes an electrolyte, a solvent and / or an additive, and the electrolyte includes any one or a combination of at least two of bis(fluorosulfonyl)imide (LiFSI), lithium trifluorosulfonyl imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalate)borate (LiBOB) and lithium oxalyldifluoroborate (LiODFB).
[0029] Optionally, the solvent includes a combination of any two or at least three of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) or ethylene carbonate (EC).
[0030] Optionally, the solvent includes any two or a combination of at least three of 1,2-dimethoxyethane (DME), 1,2-dimethoxypropane (DMP), 1,3-dioxolane (DOL), dimethoxymethane or diglyme.
[0031] Optionally, the additive includes any one of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, 4-fluoro-1,3-dioxolane-2-one (FEC) or 3-tetrafluoropropyl ether (TTE) or a combination of at least two thereof.
[0032] In a second aspect, the present invention provides a method for preparing the secondary battery as described in the first aspect, the method comprising the following steps:
[0033] (1) preparing a negative electrode from a lithium-carbon material, wherein the lithium-carbon material in the lithium-carbon material layer is composed of a cocoon formed by a linear and / or tubular carbon material and one or more lithium-containing cores contained in the cocoon, and the negative electrode preparation method comprises attaching the lithium-carbon material to a current collector by mechanical rolling, twisting, coating, spraying or stamping, or a combination of at least two of them, to form a lithium-carbon material layer;
[0034] (2) Assembling the negative electrode with the positive electrode, a separator and an electrolyte into a secondary battery.
[0035] Optionally, the coating in step (1) includes the following process:
[0036] A non-polar solvent, a conductive agent and a binder are mixed to prepare a conductive slurry, and then a lithium carbon material is added to mix to prepare a negative electrode slurry, which is coated on a current collector and baked to obtain a negative electrode sheet;
[0037] The non-polar organic solvent includes any one or a combination of at least two of alkanes with 5 to 10 carbon atoms, benzene, p-xylene or petroleum ether, preferably any one or a combination of at least two of p-xylene, n-hexane or heptane;
[0038] The binder includes any one or a combination of at least two of styrene-butadiene rubber (SBR), polyisobutylene (PIB), styrene-butadiene-styrene block copolymer (SBS) or styrene-ethylene-butylene-styrene block copolymer (SEBS);
[0039] The conductive agent includes any one of acetylene black, Ketjen black, conductive graphite, Cabot black or Super P, or a combination of at least two thereof;
[0040] The mass ratio of the conductive agent, the binder and the lithium carbon material is in the range of (1-10): (1-10): (80-98), for example, it can be 1:1:98, 1:2:97, 2:2:96, 1:5:94, 2:3:95, 3:4:93, 4:4:92, 5:5:90, 7:8:85, 10:10:80, etc., including but not limited to the above-listed ratios, preferably (2-5): (2-5): (90-96).
[0041] The non-polar organic solvent and binder do not react with the lithium-containing core, which is different from solvents such as water, N-methylpyrrolidone and binders such as PVDF in the existing process, and provides a new direction for the industrialization of powdered lithium-containing active materials.
[0042] Compared with the prior art, the present invention has at least the following beneficial effects:
[0043] (1) The secondary battery provided by the present invention has high energy density and excellent cycle performance;
[0044] (2) The present invention further improves the energy density and cycle performance of the secondary battery by selecting the type of lithium-containing core and regulating parameters such as the thickness ratio of the lithium-carbon material to the current collector;
[0045] (3) The preparation method provided by the present invention is simple to operate and has high production efficiency. In particular, the coating process is different from the existing process, which provides a new idea for the industrialization of powdered lithium-containing active materials. DETAILED DESCRIPTION
[0046] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0047] Example 1
[0048] This embodiment provides a secondary battery, wherein the positive electrode active material of the secondary battery is lithium iron phosphate, the negative electrode active material is a lithium carbon material, the electrolyte is 1 mol / L LiPF6, and the solvent is a mixture of EC, DMC and EMC in a volume ratio of 1:1:1.
[0049] The method for preparing the secondary battery comprises the following steps:
[0050] (1) Lithium iron phosphate, acetylene black, and PVDF were mixed in a mass ratio of 8:1:1, with N-methylpyrrolidone as the solvent, to prepare a slurry, which was then coated on a 10 μm aluminum foil surface and dried to obtain a positive electrode;
[0051] (2) using a roller press to roll a lithium carbon material onto a surface of a 10 μm carbon nanotube paper to prepare a negative electrode, wherein the mass ratio of the single-walled carbon nanotube to the metal lithium powder in the lithium carbon material is 1:50, the thickness ratio of the lithium carbon material layer to the carbon nanotube paper is 5:1, the N / P ratio is adjusted to 3, and the positive electrode, the negative electrode and the electrolyte are encapsulated using a CR2025 positive and negative electrode shell to obtain a secondary battery;
[0052] The preparation method of the lithium carbon material is as follows:
[0053] Weigh 1g of single-walled carbon nanotubes (OxyAl) with a mass fraction of 3% into a beaker, add 52g of n-hexane, disperse at 12000rpm for 2min, add 1.5g of metal lithium powder with an average particle size of 20μm, mix at 12000rpm for 2min. Filter by suction, heat to remove n-hexane, and obtain lithium-carbon material.
[0054] The secondary battery is cycled at 0.5C with a voltage range of 2.7-4.0V, an initial discharge capacity of 149.58mAh / g, and can be stably cycled for 380 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0055] Example 2
[0056] This embodiment provides a secondary battery, wherein the positive electrode active material of the secondary battery is lithium iron phosphate, the negative electrode active material is a lithium carbon material, the electrolyte is 1 mol / L LiTFSI, and the solvent is a mixture of DOL and DME in a volume ratio of 1:1.
[0057] The method for preparing the secondary battery comprises the following steps:
[0058] (1) NCM811, acetylene black and PVDF were mixed in a mass ratio of 8:1:1, with N-methylpyrrolidone as the solvent to prepare a slurry, which was then coated on a 10 μm aluminum foil surface and dried to obtain a positive electrode;
[0059] (2) using a roller press to roll a lithium-carbon material onto a surface of a 6 μm perforated copper foil to prepare a negative electrode, wherein the mass ratio of carbon nanofibers to metallic lithium powder in the lithium-carbon material is 1:500, the thickness ratio of the lithium-carbon material layer to the perforated copper foil is 50:1, the N / P ratio is adjusted to 5.5, and the positive electrode, the negative electrode and the electrolyte are encapsulated using CR2025 positive and negative electrode shells to obtain a secondary battery;
[0060] The preparation method of the lithium carbon material is as follows:
[0061] Weigh 0.1 g of carbon nanofibers with a mass fraction of 3% (Tianjin Xidian Chemical Technology Co., Ltd.) in a beaker, add 52 g of p-xylene, disperse at 10,000 rpm for 5 min, add 1.5 g of metal lithium powder with an average particle size of 10 μm, mix at 12,000 rpm for 2 min, filter, heat to remove p-xylene, and obtain lithium-carbon material.
[0062] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 187.52mAh / g, and can be stably cycled for 280 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0063] Example 3
[0064] This embodiment provides a secondary battery, wherein the positive electrode active material of the secondary battery is sublimated sulfur, the negative electrode active material is a lithium carbon material, the electrolyte is 1 mol / L LiClO4, and the solvent is a mixture of DOL and DME in a volume ratio of 1:1.
[0065] The method for preparing the secondary battery comprises the following steps:
[0066] (1) Sublimed sulfur, acetylene black, and PVDF are mixed in a mass ratio of 7:2:1, with N-methylpyrrolidone as the solvent, to prepare a slurry, which is then coated on the surface of 10 μm nickel foam and dried to obtain a positive electrode;
[0067] (2) rolling the lithium carbon material onto the surface of nickel foam by a roller press to prepare a negative electrode, wherein the thickness of the nickel foam after rolling is 10 μm, the mass ratio of carbon nanofibers to metal lithium powder in the lithium carbon material is 1:1000, the ratio of the lithium carbon material layer to the thickness of the nickel foam after rolling is 100:1, the N / P ratio is adjusted to 3, and the positive electrode, the negative electrode and the electrolyte are encapsulated by using CR2025 positive and negative electrode shells to obtain a secondary battery;
[0068] The preparation method of the lithium carbon material is as follows:
[0069] Weigh 0.1 g of carbon nanofibers with a mass fraction of 3% (Tianjin Xidian Chemical Technology Co., Ltd.) in a beaker, add 52 g of p-xylene, disperse at 10,000 rpm for 5 min, add 3.0 g of metal lithium powder with an average particle size of 50 μm, mix at 12,000 rpm for 2 min, filter, heat to remove p-xylene, and obtain lithium-carbon material.
[0070] The secondary battery is cycled at 0.1C with a voltage range of 1.5-3.0V, an initial discharge capacity of 996.34mAh / g, and can be stably cycled for 53 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0071] Example 4
[0072] Compared with Example 2, the only difference is that the electrolyte solvent is replaced with a mixture of DME and DMP in a volume ratio of 1:1, and 10 wt% of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether is added. The other conditions are the same as those in Example 2.
[0073] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 185.53mAh / g, and can be stably cycled for 353 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0074] Example 5
[0075] Compared with Example 2, the only difference is that the metallic lithium powder is replaced by lithium-boron alloy powder.
[0076] The secondary battery was cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 185.72mAh / g, and could stably cycle 313 times when the discharge capacity was 80% of the initial discharge capacity.
[0077] Example 6
[0078] Compared with Example 2, the only difference is that the metallic lithium powder is replaced by lithium-tin-silver alloy powder.
[0079] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 185.16mAh / g, and can be stably cycled for 383 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0080] Example 7
[0081] Compared with Example 2, the only difference is that the preparation method of the negative electrode is different, and the other conditions are the same as those of Example 2. The negative electrode is prepared by a coating method:
[0082] Lithium carbon material, acetylene black and PIB were mixed into slurry in a mass ratio of 90:5:5, with heptane as the solvent and a solid content of 40%, and then coated on the surface of a 6 μm perforated copper foil and dried to obtain a negative electrode.
[0083] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 188.34mAh / g, and can be stably cycled for 295 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0084] Comparative Example 1
[0085] Compared with Example 2, the only difference is that the lithium carbon material is replaced by pure metallic lithium powder, and the other conditions are the same as those in Example 2.
[0086] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 186.88mAh / g, and can be stably cycled for 81 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0087] Comparative Example 2
[0088] Compared with Example 2, the only difference is that the lithium carbon material is replaced by metal lithium foil, and the other conditions are the same as those in Example 2.
[0089] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 187.05mAh / g, and can be stably cycled for 96 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0090] Comparative Example 3
[0091] Compared with Example 2, the only difference is that the lithium carbon material is replaced by a mixture of carbon nanofibers and metallic lithium powder randomly distributed, and the other conditions are the same as those of Example 2;
[0092] The preparation method of the mixture is as follows: dispersing carbon nanofibers in n-hexane, adding metal lithium powder, then stirring and mixing evenly with magnetic force, filtering, and drying to obtain the mixture.
[0093] The secondary battery is cycled at 2C with a voltage range of 3.0-4.3V, an initial discharge capacity of 186.62mAh / g, and can be stably cycled for 112 cycles when the discharge capacity is 80% of the initial discharge capacity.
[0094] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A secondary battery containing a lithium-carbon material, characterized in that: The secondary battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a current collector and a lithium-carbon material layer arranged on the surface of the current collector, and the lithium-carbon material in the lithium-carbon material layer consists of a cocoon formed by linear and / or tubular carbon materials and one or more lithium-containing cores contained in the cocoon.
2. The secondary battery according to claim 1, characterized in that: The lithium-containing core comprises metal lithium powder and / or metal lithium alloy powder, preferably metal lithium alloy powder, and the average particle size of the metal lithium powder and / or metal lithium alloy powder is 1-100 microns, preferably 1-30 microns; Preferably, the metallic lithium alloy powder comprises a binary lithium alloy and / or a ternary lithium alloy, the binary lithium alloy powder comprises any one of a lithium boron alloy, a lithium silver alloy, a lithium indium alloy, a lithium silicon alloy, a lithium aluminum alloy or a lithium tin alloy, or a combination of at least two thereof; the ternary lithium alloy powder comprises any one of a lithium tin silver alloy, a lithium silver silicon alloy or a lithium boron zinc alloy, or a combination of at least two thereof.
3. The secondary battery according to claim 1 or 2, characterized in that: The current collector includes any one of copper foil, PET copper foil, foam copper, perforated copper foil, nickel foil, foam nickel, perforated nickel foil, carbon nanotube paper or graphene paper, or a combination of at least two thereof.
4. The secondary battery according to any one of claims 1 to 3, characterized in that: The thickness ratio of the lithium-carbon material layer to the current collector is (1-100):1, preferably (5-80):
1.
5. The secondary battery according to any one of claims 1 to 4, characterized in that: The linear and / or tubular carbon material comprises any one or a combination of at least two of single-walled carbon nanotubes, few-walled carbon nanotubes, multi-walled carbon nanotubes, doped carbon nanotubes, carbon nanofibers or doped carbon nanofibers; Preferably, the doping element in the doped carbon nanotubes and / or doped carbon nanofibers includes any one or a combination of at least two of nitrogen, oxygen, silver, silicon, tin or zinc; Preferably, the mass ratio of the linear and / or tubular carbon material to the lithium-containing core is 1:(50-1000), preferably 1:(100-500).
6. The secondary battery according to any one of claims 1 to 5, characterized in that: The positive electrode active material includes any one of elemental sulfur, oxygen, lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, or a combination of at least two thereof, preferably lithium iron phosphate and / or lithium nickel cobalt manganese oxide.
7. The secondary battery according to any one of claims 1 to 6, characterized in that: The ratio of the negative electrode capacity to the positive electrode capacity of the secondary battery (N / P ratio) is 2-6, preferably 3-5.
8. The secondary battery according to any one of claims 1 to 7, characterized in that: The electrolyte comprises an electrolyte, a solvent and / or an additive; Preferably, the electrolyte comprises any one or a combination of at least two of bis(fluorosulfonyl)imide (LiFSI), lithium trifluorosulfonyl imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalate)borate (LiBOB) and lithium oxalyldifluoroborate (LiODFB); Preferably, the solvent includes any one of dimethyl carbonate, ethyl methyl carbonate or ethylene carbonate or a combination of at least two thereof; or the solvent includes any one of 1,2-dimethoxyethane, 1,2-dimethoxypropane, 1,3-dioxolane, dimethoxymethane or diethylene glycol dimethyl ether or a combination of at least two thereof; Preferably, the additive includes any one of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, 4-fluoro-1,3-dioxolane-2-one or 3-tetrafluoropropyl ether, or a combination of at least two thereof.
9. A method for preparing a secondary battery as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: (1) preparing a negative electrode from a lithium-carbon material, wherein the lithium-carbon material in the lithium-carbon material layer is composed of a cocoon formed by a linear and / or tubular carbon material and one or more lithium-containing cores contained in the cocoon, and the negative electrode preparation method comprises attaching the lithium-carbon material to a current collector by mechanical rolling, twisting, coating, spraying or stamping, or a combination of at least two of them, to form a lithium-carbon material layer; (2) Assembling the negative electrode with the positive electrode, a separator and an electrolyte into a secondary battery.
10. The method according to claim 9, characterized in that The coating in step (1) includes the following processes: The non-polar solvent, the conductive agent and the binder are mixed to prepare a conductive slurry, and then the lithium carbon material is added to mix to prepare a negative electrode slurry, which is coated on the current collector and baked to obtain a negative electrode sheet; IB231883 The non-polar solvent includes any one or a combination of at least two of liquid alkanes with 5 to 10 carbon atoms, benzene, p-xylene or petroleum ether, preferably any one or a combination of at least two of p-xylene, n-hexane or heptane; The conductive agent includes any one of acetylene black, Ketjen black, conductive graphite, Cabot black or Super P, or a combination of at least two thereof; The binder comprises any one or a combination of at least two of styrene-butadiene rubber, polyisobutylene, styrene-butadiene-styrene block copolymer or styrene-ethylene-butylene-styrene block copolymer; The mass ratio of the conductive agent, the binder and the lithium carbon material is in the range of (1-10): (1-10): (80-98), preferably (2-5): (2-5): (90-96).
Citation Information
Patent Citations
Process of production of a stabilized lithium metal powder for Li-ion application
CN101213039B