Powder falling prevention pretreatment method for positive plate of nickel-metal hydride battery
By soaking the positive electrode sheet of the nickel-metal hydride battery in glue and drying it, the problem of cracks and powdering of the conductive coating during the softening, trimming and winding processes of the positive electrode sheet is solved, and the life and performance of the battery are improved.
Patent Information
- Application Number
- CN202410673598.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-18
AI Technical Summary
Nickel-metal hydride battery cathode sheets are prone to cracks during the softening, trimming and winding processes, causing the conductive coating to powder and fall off, affecting the life and performance of the battery.
The nickel-metal hydride battery positive electrode sheet is pre-treated to prevent powder loss, including soaking the positive electrode sheet in glue to form a glue-impregnated electrode sheet, and then baking it in a drying equipment to dry the glue into a film and increase the flexibility of the positive electrode sheet. And reduce conductive coating powdering and falling off.
Through the glue wrapping and drying process, the flexibility of the positive electrode sheet is improved, cracks and conductive coating powdering are reduced, the battery life is extended and the battery is maintained in good condition.
Smart Images

Figure CN118800883A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nickel-hydrogen battery pole piece production, and in particular to a nickel-hydrogen battery positive pole piece anti-powdering pretreatment method. Background Art
[0002] Nickel-metal hydride batteries are a new generation of high-energy secondary batteries after nickel-cadmium batteries. They are favored by people because of their high capacity, high power, and pollution-free characteristics. They are one of the important development directions of secondary batteries today. Nowadays, nickel-metal hydride batteries are increasingly used in communications and digital products, power tools, instruments, toys, and other fields. However, with the advancement of social modernization, people's requirements for rechargeable batteries are getting higher and higher, mainly reflected in the life, storage performance, and safety performance of rechargeable batteries. However, the positive electrode is prone to cracks during softening, cutting edges, and winding, which makes the conductive coating on its surface easy to powderize. After the conductive coating is powderized, it will fall off the surface of the positive electrode, resulting in low voltage, low capacity, and low cycle life of the battery. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a nickel-hydrogen battery positive electrode sheet anti-powder loss pretreatment method that can increase the flexibility of the nickel-hydrogen battery positive electrode sheet and reduce the occurrence of cracks in the positive electrode sheet.
[0004] The purpose of this disclosure is achieved through the following technical solutions:
[0005] A method for pretreating a nickel-hydrogen battery positive electrode sheet to prevent powder from falling off, comprising:
[0006] Get the positive electrode;
[0007] Soaking the positive electrode sheet in glue to obtain a glue-impregnated electrode sheet;
[0008] Placing the dipped electrode in a drying device to obtain a dried electrode;
[0009] The drying electrode sheets are placed in a packing box to collect the drying electrode sheets.
[0010] In one embodiment, the positive electrode sheet is immersed in glue to obtain a glue-impregnated electrode sheet, comprising:
[0011] Placing the positive electrode sheet on a conveyor belt of an automatic glue dipping machine to convey the positive electrode sheet to a glue dipping area of the automatic glue dipping machine;
[0012] The positive electrode sheet is soaked for a predetermined soaking time to obtain the resin-impregnated electrode sheet.
[0013] In one embodiment, the predetermined soaking time is 2 seconds to 5 seconds.
[0014] In one embodiment, placing the dipped electrode in a drying device to obtain a dried electrode comprises:
[0015] Placing the dipped electrode on the conveyor belt of the drying equipment to convey the dipped electrode to the drying area of the drying equipment;
[0016] The dipped electrode is dried for a predetermined baking time to obtain the dried electrode.
[0017] In one embodiment, the predetermined baking time is 20 seconds to 40 seconds.
[0018] In one embodiment, the temperature of the drying zone is 100°C to 125°C.
[0019] In one embodiment, the positive electrode sheet is immersed in glue to obtain the dipped electrode sheet, and the method further comprises:
[0020] The glue solution is mixed with pure water in a predetermined ratio to obtain the glue.
[0021] In one embodiment, the predetermined ratio of the glue solution to the pure water is 1:10.
[0022] In one embodiment, before placing the drying electrode pieces in a packing box to collect the drying electrode pieces, the method further includes:
[0023] Placing the drying electrode on a work surface;
[0024] The drying electrodes are stacked to arrange the drying electrodes into groups.
[0025] In one embodiment, after placing the drying electrode pieces in a packing box to collect the drying electrode pieces, the method further comprises:
[0026] Place the label in the packaging box.
[0027] Compared with the prior art, the present invention has at least the following advantages:
[0028] The above-mentioned nickel-hydrogen battery positive electrode plate anti-powdering pretreatment method, by immersing the positive electrode plate in the glue, can make the glue adhere to the positive electrode plate, so that the surface of the positive electrode plate can be wrapped by the glue to obtain the dipped electrode plate, and then the dipped electrode plate is placed in the drying equipment, and the dipped electrode plate is baked by the drying equipment to obtain a dried electrode plate, and finally the dried electrode plate is placed in a packing box to collect the dried electrode plate. The dipped electrode plate is baked by the drying equipment so that the glue on the surface of the positive electrode plate is dried to form a film, and the surface of the positive electrode plate becomes more flexible after being wrapped by the glue, and is less likely to crack during softening, cutting edges and winding processes, thereby reducing the occurrence of powdering of the conductive coating on the surface of the positive electrode plate. At the same time, since the surface of the positive electrode plate is wrapped with the glue, the conductive coating is not easy to fall off from the surface of the positive electrode plate after powdering, thereby ensuring that the battery remains in a good state. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a flow chart of a method for pre-treating a nickel-hydrogen battery positive electrode sheet to prevent powder from falling off according to an embodiment of the present disclosure;
[0031] Figure 2 for Figure 1 The process flow chart of the method for pretreating the positive electrode sheet of a nickel-hydrogen battery to prevent powder loss is shown. DETAILED DESCRIPTION
[0032] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.
[0033] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0035] In order to better understand the technical solutions and beneficial effects of the present invention, the present invention is further described in detail below in conjunction with specific embodiments:
[0036] The present disclosure provides a pretreatment method for preventing powder loss of a nickel-hydrogen battery positive electrode sheet, comprising: obtaining a positive electrode sheet; soaking the positive electrode sheet in glue to obtain a glue-impregnated electrode sheet; placing the glue-impregnated electrode sheet in a drying device to obtain a dried electrode sheet; placing the dried electrode sheet in a packing box to collect the dried electrode sheet.
[0037] It can be understood that by immersing the positive electrode sheet in the glue, the glue can be attached to the positive electrode sheet, so that the surface of the positive electrode sheet can be wrapped by the glue to obtain the dipped electrode sheet, and then the dipped electrode sheet is placed in the drying equipment, and the dipped electrode sheet is baked by the drying equipment to obtain a dried electrode sheet, and finally the dried electrode sheet is placed in a packing box to collect the dried electrode sheet. The dipped electrode sheet is baked by the drying equipment so that the glue on the surface of the positive electrode sheet is dried to form a film. The surface of the positive electrode sheet becomes more flexible after being wrapped by the glue, and is less likely to crack during softening, cutting edges and winding, thereby reducing the occurrence of powdering of the conductive coating on the surface of the positive electrode sheet. At the same time, since the surface of the positive electrode sheet is wrapped with the glue, the conductive coating is not easy to fall off from the surface of the positive electrode sheet after powdering, thereby ensuring that the battery remains in a good state.
[0038] See also Figure 1 and Figure 2 As shown, the nickel-hydrogen battery positive electrode sheet anti-powdering pretreatment method includes part or all of the following steps:
[0039] S100, obtaining a positive electrode sheet.
[0040] In this embodiment, the positive electrode sheet is the positive electrode sheet that has been spot-welded with the tab tape and softened, that is, the positive electrode sheet is coated with a conductive coating.
[0041] S200, soaking the positive electrode sheet in glue to obtain a glue-impregnated electrode sheet.
[0042] In this embodiment, by immersing the positive electrode sheet in the glue, the glue can be attached to the positive electrode sheet, so that the surface of the positive electrode sheet can be wrapped by the glue to obtain the glue-impregnated electrode sheet.
[0043] S300, placing the dipped electrode in a drying device to obtain a dried electrode.
[0044] In this embodiment, by placing the dipped electrode in the drying device, the glue on the surface of the positive electrode is dried to form a film, and the surface of the positive electrode is wrapped with the glue to make it more flexible, and less likely to crack during softening, cutting edges and winding, thereby reducing the occurrence of powdering of the conductive coating on the surface of the positive electrode. At the same time, since the surface of the positive electrode is wrapped with the glue, the conductive coating is not likely to fall off the surface of the positive electrode after powdering, thereby ensuring that the battery remains in a good state.
[0045] S400, placing the drying electrode sheets in a packing box to collect the drying electrode sheets.
[0046] In this embodiment, the drying electrodes are finally placed in a packing box so that the drying electrodes can be collected and it is more convenient for operators to carry the packing box.
[0047] In one embodiment, S200, immersing the positive electrode sheet in glue to obtain a glue-impregnated electrode sheet, comprises:
[0048] S210, placing the positive electrode sheet on a conveyor belt of an automatic glue dipping machine to convey the positive electrode sheet to a glue dipping area of the automatic glue dipping machine; wherein the glue dipping area contains the glue;
[0049] S220, soaking the positive electrode sheet for a predetermined soaking time to obtain the resin-impregnated electrode sheet.
[0050] In this embodiment, the positive electrode sheet is placed on the conveyor belt of the automatic glue dipping machine so that the positive electrode sheet can move with the conveyor belt of the automatic glue dipping machine. The conveyor belt of the automatic glue dipping machine conveys the positive electrode sheet to the glue dipping area of the automatic glue dipping machine, so that the positive electrode sheet can be immersed in the glue in the glue dipping area. After the positive electrode sheet is immersed in the glue dipping area for a predetermined immersion time, the glue can adhere to the positive electrode sheet, thereby wrapping the surface of the positive electrode sheet to obtain the dipped electrode sheet.
[0051] Specifically, the predetermined soaking time is 2 seconds to 5 seconds. It can be understood that by soaking the positive electrode sheet in the glue dipping area for 2 seconds to 5 seconds, the glue can be absorbed and wrapped around the positive electrode sheet while avoiding the glue adsorbed by the positive electrode sheet being too thick, thereby reducing the conductive effect of the positive electrode sheet. Among them, the predetermined soaking time can be 2 seconds, 3 seconds or 5 seconds, which is not limited here, and those skilled in the art can adjust it according to the thickness of the glue adsorbed by the positive electrode sheet.
[0052] In another embodiment, placing the positive electrode sheet on the conveyor belt of the automatic dipping machine in S210 specifically includes the following steps:
[0053] S211, starting the conveyor belt of the automatic glue dipping machine to move the conveyor belt of the automatic glue dipping machine toward the glue dipping area of the automatic glue removal machine;
[0054] S212, when the conveyor belt of the automatic dipping machine moves a first predetermined distance, placing one of the positive electrode sheets on the conveyor belt of the automatic dipping machine;
[0055] S213, determining whether the number of the positive electrode sheets on the rack is equal to zero;
[0056] S214, when the number of the positive electrode sheets is not equal to zero, executing step S212;
[0057] S215. When the number of the positive electrode sheets is equal to zero, execute step S220.
[0058] It can be understood that by starting the conveyor belt of the automatic glue dipping machine, the conveyor belt of the automatic glue dipping machine can be moved to the glue dipping area of the automatic glue removal machine. When the conveyor belt of the automatic glue dipping machine moves a predetermined distance, by placing one of the positive electrode sheets on the conveyor belt of the automatic glue dipping machine, one of the positive electrode sheets is placed at a first predetermined position of the conveyor belt of the automatic glue dipping machine. By judging whether the number of the positive electrode sheets on the material rack is equal to zero, when the number of the positive electrode sheets on the material rack is not equal to zero, it means that there are still positive electrode sheets that have not been placed on the conveyor belt of the automatic glue dipping machine. After the conveyor belt of the automatic glue dipping machine moves the first predetermined distance, by placing another positive electrode sheet Place it on the conveyor belt of the automatic glue dipping machine, so that another positive electrode sheet is placed at the second predetermined position of the conveyor belt of the automatic glue dipping machine, and finally all the positive electrode sheets are arranged in sequence along the moving direction of the conveyor belt of the automatic glue dipping machine. When the number of the positive electrode sheets on the material rack is zero, it means that all the positive electrode sheets are placed on the conveyor belt of the automatic glue dipping machine. After that, the conveyor belt of the automatic glue dipping machine conveys the positive electrode sheets to the glue dipping area of the automatic glue dipping machine, so that all the positive electrode sheets can be moved and immersed in the glue dipping area of the automatic glue dipping machine at one time, which can effectively improve the efficiency of the glue dipping area of the automatic glue dipping machine in immersing and wrapping the positive electrode sheets.
[0059] In one embodiment, the first predetermined distance is greater than the length of the positive electrode sheet in the moving direction of the conveyor belt of the automatic glue dipping machine, which means that after the positive electrode sheet is placed on the conveyor belt of the automatic glue dipping machine, there is a gap between the two adjacent positive electrode sheets. It can be understood that by making the first predetermined distance greater than the length of the positive electrode sheet in the moving direction of the conveyor belt of the automatic glue dipping machine, after the positive electrode sheet is placed on the conveyor belt of the automatic glue dipping machine, a gap can be maintained between the two adjacent positive electrode sheets to avoid overlapping placement between the two adjacent positive electrode sheets. If the two adjacent positive electrode sheets are placed overlappingly, when the positive electrode sheet is conveyed to the glue dipping area of the automatic glue dipping machine with the conveyor belt of the automatic glue dipping machine, the two adjacent positive electrode sheets will be wrapped together by glue and adhered together, which will result in the need to separate the mutually adhered positive electrode sheets in the future, making the operation process more time-consuming and labor-intensive.
[0060] In another embodiment, multiple predetermined placement frames are drawn at even intervals along the moving direction of the conveyor belt of the automatic glue dipping machine and a camera is added to solve the problem that in the process of placing the positive electrode sheet, after the conveyor belt of the automatic glue dipping machine moves the first predetermined distance, it is difficult to place the positive electrode sheet on the conveyor belt of the automatic glue dipping machine in a timely and accurate manner. If the previous positive electrode sheet is not accurately placed on the conveyor belt of the automatic glue dipping machine, it will affect the placement of subsequent positive electrode sheets in turn, making the gap between subsequent positive electrode sheets smaller, and further making it possible for two adjacent positive electrode sheets to be wrapped together by glue and adhered together.
[0061] S212, when the conveyor belt of the automatic glue dipping machine moves a first predetermined distance, placing one of the positive electrode sheets on the conveyor belt of the automatic glue dipping machine, specifically comprising the following steps:
[0062] When the conveyor belt of the automatic dipping machine moves, obtaining a placement frame distribution image on the conveyor belt;
[0063] Acquire the horizontal coordinate of the center of the placement box according to the placement box distribution image;
[0064] Calculate the difference between the horizontal coordinate of the center of the placement frame and the horizontal coordinate of the center of the preset position to obtain the lateral distance difference of the center movement of the placement frame, wherein the preset position is the position of the placement frame after it moves the first distance along the conveyor belt of the automatic glue dipping machine, and the horizontal coordinate of the center of the preset position is the horizontal coordinate of the center of the position of the placement frame after it moves the first distance along the conveyor belt of the automatic glue dipping machine.
[0065] Detecting whether the horizontal distance difference of the center of the placement frame is greater than the preset horizontal distance difference;
[0066] When the lateral distance difference of the center of the placement frame is greater than the preset lateral distance difference, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to move in the reverse direction to reduce the distance between the placement frame and the preset position;
[0067] Place one of the positive electrode sheets in the placement frame.
[0068] In this embodiment, the camera is installed on the automatic glue dipping machine, and the camera is set toward the conveyor belt of the automatic glue dipping machine, so that the conveyor belt of the automatic glue dipping machine can be photographed by the camera, and then the placement frame distribution image on the conveyor belt is obtained, and the placement frame distribution image is used to show the position distribution of the placement frame on the conveyor belt, that is, the current position of the placement frame on the conveyor belt of the automatic glue dipping machine can be obtained, by comparing the current position of the placement frame on the conveyor belt of the automatic glue dipping machine and the preset position, the lateral distance difference of the center movement of the placement frame is greater than the preset lateral distance difference, indicating that the conveyor belt of the automatic glue dipping machine has moved too far toward the glue dipping area of the automatic glue removal machine, that is, the placement frame deviates from the preset position, and the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to move in the reverse direction, which can effectively reduce the distance between the placement frame and the preset position, thereby reducing the degree of deviation of the placement frame, so that the placement frame is further close to the preset position. For example, the preset lateral distance difference may be 0 mm, that is, when the preset lateral distance difference is greater than 0 mm, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to move in reverse, so that the placement frame is located at the preset position. The placement frame can be located at the preset position simply by comparing the lateral distance difference of the center movement of the placement frame to be greater than the preset lateral distance difference. Finally, the positive electrode sheets are placed one by one in the placement area so that the positive electrode sheets are evenly spaced on the conveyor belt of the automatic glue dipping machine.
[0069] In another embodiment, when the lateral distance difference of the center movement of the placement frame is less than the preset lateral distance difference, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to move forward to increase the distance between the placement frame and the preset position;
[0070] Place one of the positive electrode sheets in the placement frame.
[0071] In this embodiment, the current position of the placement frame on the conveyor belt of the automatic glue dipping machine is obtained through a camera, and then by comparing the current position of the placement frame on the conveyor belt of the automatic glue dipping machine and the preset position, the lateral distance difference of the center movement of the placement frame is smaller than the preset lateral distance difference, indicating that the conveyor belt of the automatic glue dipping machine has moved too close to the glue dipping area of the automatic glue removal machine, that is, the placement frame deviates from the preset position. By controlling the forward movement of the conveyor belt of the automatic glue dipping machine by the automatic glue dipping machine, the distance between the placement frame and the preset position can be effectively increased, thereby reducing the degree of deviation of the placement frame, so that the placement frame is further closer to the preset position. For example, the preset lateral distance difference may be 0 mm, that is, when the preset lateral distance difference is less than 0 mm, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to move forward, so that the placement frame is located at the preset position. The placement frame can be located at the preset position simply by comparing the lateral distance difference of the center movement of the placement frame with the preset lateral distance difference. Finally, the positive electrode sheets are placed one by one in the placement area so that the positive electrode sheets are evenly spaced on the conveyor belt of the automatic glue dipping machine.
[0072] In one embodiment, the placement frame is the same size as the positive electrode sheet, and one of the positive electrode sheets is placed in the placement frame, and then the steps include:
[0073] Acquire a distribution image of the positive electrode sheets on the conveyor belt;
[0074] Acquire the abscissa of the center of the positive electrode sheet according to the positive electrode sheet distribution image;
[0075] Obtaining the horizontal coordinate of the center of the positive electrode sheet and the horizontal coordinate of the center of the placement frame to obtain the horizontal distance difference of the center movement of the positive electrode sheet;
[0076] Detecting whether the lateral distance difference of the center movement of the positive electrode sheet is greater than the preset lateral distance difference of the positive electrode sheet;
[0077] When the lateral distance difference of the center movement of the positive electrode sheet is greater than the preset lateral distance difference of the positive electrode sheet, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to stop moving, so as to stop conveying the positive electrode sheet;
[0078] Adjusting the position of the positive electrode sheet in the placement frame to reduce the distance between the center position of the positive electrode sheet and the center of the placement frame;
[0079] The automatic glue dipping machine controls the movement of the conveyor belt of the automatic glue dipping machine so that the positive electrode sheet continues to be conveyed to the glue dipping area of the automatic glue removal machine.
[0080] In this embodiment, a distribution image of the positive electrode sheets on the conveyor belt is obtained by a camera, and the distribution image of the positive electrode sheets is used to display the position distribution of the positive electrode sheets on the conveyor belt, that is, to obtain the position of the positive electrode sheets placed on the conveyor belt of the automatic glue dipping machine, and then by comparing the lateral distance difference of the center movement of the positive electrode sheets with the preset lateral distance difference of the positive electrode sheets, the lateral distance difference of the center movement of the positive electrode sheets is greater than the preset lateral distance difference of the positive electrode sheets, indicating that the center position of the positive electrode sheets is too far from the center position of the placement frame, that is, the center position of the positive electrode sheets deviates from the center position of the placement frame, and the automatic glue dipping machine is controlled to stop the conveyor belt of the automatic glue dipping machine, so as to facilitate the readjustment of the position of the positive electrode sheets, thereby reducing the distance between the center position of the positive electrode sheets and the center position of the placement frame, so as to accurately place the positive electrode sheets in the placement frame. For example, the preset lateral distance difference of the positive electrode sheet can be 0mm, that is, when the lateral distance difference of the center movement of the positive electrode sheet is greater than 0mm, the automatic dipping machine controls the conveyor belt of the automatic dipping machine to stop moving, so as to facilitate the adjustment of the position of the positive electrode sheet relative to the placement frame, so that the center position of the positive electrode sheet coincides with the center position of the placement frame, and then the positive electrode sheets can be evenly spaced on the conveyor belt of the automatic dipping machine. Finally, the automatic dipping machine controls the movement of the conveyor belt of the automatic dipping machine, so that the positive electrode sheet can continue to be conveyed to the dipping area of the automatic glue removal machine.
[0081] When the lateral distance difference of the center movement of the positive electrode sheet is less than the preset lateral distance difference of the positive electrode sheet, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to stop moving, so as to stop conveying the positive electrode sheet;
[0082] Adjusting the position of the positive electrode sheet in the placement frame to increase the distance between the center position of the positive electrode sheet and the center of the placement frame;
[0083] The automatic glue dipping machine controls the movement of the conveyor belt of the automatic glue dipping machine so that the positive electrode sheet continues to be conveyed to the glue dipping area of the automatic glue removal machine.
[0084] In this embodiment, the position of the positive electrode sheet placed on the conveyor belt of the automatic glue dipping machine is obtained by a camera, and then the lateral distance difference of the center movement of the positive electrode sheet can be compared with the preset lateral distance difference of the positive electrode sheet. If the lateral distance difference of the center movement of the positive electrode sheet is smaller than the preset lateral distance difference of the positive electrode sheet, it indicates that the center position of the positive electrode sheet is too close to the center position of the placement frame, that is, it indicates that the center position of the positive electrode sheet deviates from the center position of the placement frame. The automatic glue dipping machine is controlled to stop the conveyor belt of the automatic glue dipping machine, so as to facilitate the readjustment of the position of the positive electrode sheet, thereby expanding the distance between the center position of the positive electrode sheet and the center position of the placement frame, so as to accurately place the positive electrode sheet in the placement frame. For example, the preset lateral distance difference of the positive electrode sheet can be 0mm, that is, when the lateral distance difference of the center movement of the positive electrode sheet is less than 0mm, the automatic glue dipping machine controls the conveyor belt of the automatic glue dipping machine to stop moving, so as to facilitate the adjustment of the position of the positive electrode sheet relative to the placement frame, so that the center position of the positive electrode sheet coincides with the center position of the placement frame, and then the positive electrode sheets can be evenly spaced on the conveyor belt of the automatic glue dipping machine. Finally, the automatic glue dipping machine controls the movement of the conveyor belt of the automatic glue dipping machine, so that the positive electrode sheet can continue to be conveyed to the glue dipping area of the automatic glue removal machine.
[0085] In another embodiment, when the lateral distance of the center movement of the positive electrode sheet is equal to the preset lateral distance of the positive electrode sheet, the automatic dipping machine controls the conveyor belt of the automatic dipping machine to move so that the positive electrode sheet is conveyed to the dipping area of the automatic glue removal machine.
[0086] The position of the positive electrode sheet placed on the conveyor belt of the automatic glue dipping machine is obtained through a camera, and then by comparing the lateral distance difference of the center movement of the positive electrode sheet with the preset lateral distance difference of the positive electrode sheet, the lateral distance difference of the center movement of the positive electrode sheet is equal to the preset lateral distance difference of the positive electrode sheet, indicating that the center position of the positive electrode sheet is aligned with the center position of the placement frame, that is, the position of the positive electrode sheet placed on the placement frame is accurate, that is, there is no need to adjust the position of the positive electrode sheet. For example, the preset lateral distance difference of the positive electrode sheet can be 0mm, that is, when the lateral distance difference of the center movement of the positive electrode sheet is equal to 0mm, the center position of the positive electrode sheet coincides with the center position of the placement frame. At this time, the positive electrode sheet is accurately placed on the placement frame, and there is no need to adjust the position of the positive electrode sheet. The automatic glue dipping machine is directly used to control the movement of the conveyor belt of the automatic glue dipping machine to convey the positive electrode sheet to the glue dipping area of the automatic glue removal machine.
[0087] In one of the embodiments, a recess is formed in the placement frame, and the placement groove is used to lay the positive electrode sheet flat, so as to solve the problem that after the positive electrode sheet is placed on the placement frame, when the positive electrode sheet is conveyed to the dipping area of the automatic dipping machine along the conveyor belt of the automatic dipping machine, the positive electrode sheet is hindered by the glue in the dipping area of the automatic dipping machine and slips relative to the conveyor belt of the automatic dipping machine. The positive electrode sheet is easy to slip in the dipping area of the automatic dipping machine and touch another adjacent positive electrode sheet, so that the two adjacent positive electrode sheets are still easily wrapped by glue and adhered together.
[0088] Placing a positive electrode sheet in the placement frame includes:
[0089] One of the positive electrode sheets is laid flat in the containing groove.
[0090] It can be understood that by laying the positive electrode sheet flat in the receiving groove, when the conveyor belt of the automatic glue dipping machine moves, the positive electrode sheet in the receiving groove is constrained by the receiving groove, so that it can move more synchronously with the conveyor belt of the automatic glue dipping machine, and can offset the obstruction of the glue to the positive electrode sheet, thereby reducing the occurrence of the positive electrode sheet slipping in the glue dipping area of the automatic glue dipping machine.
[0091] In one embodiment, S300, placing the dipped electrode in a drying device to obtain a dried electrode, includes:
[0092] S310, placing the dipped electrode on the conveyor belt of the drying equipment to convey the dipped electrode to the drying area of the drying equipment;
[0093] S320, drying the dipped electrode for a predetermined baking time to obtain the dried electrode.
[0094] In this embodiment, the dipped electrode sheet is placed on the conveyor belt of the drying equipment so that the positive electrode sheet can move with the conveyor belt of the drying equipment. The conveyor belt of the drying equipment conveys the positive electrode sheet to the drying area of the drying equipment, so that the positive electrode sheet can be baked in the drying area of the drying equipment. After the positive electrode sheet passes through the predetermined baking time in the drying area of the drying equipment, the glue on the surface of the positive electrode sheet is dried to form a film. The surface of the positive electrode sheet becomes more flexible after being wrapped by the glue, and is less likely to crack during softening, cutting edges and winding, thereby reducing the occurrence of powdering of the conductive coating on the surface of the positive electrode sheet. At the same time, since the surface of the positive electrode sheet is wrapped with the glue, the conductive coating is not easy to fall off from the surface of the positive electrode sheet after powdering, thereby ensuring that the battery remains in a good state. The dipped electrode sheet is obtained after passing through the drying area of the drying equipment. The dipped electrode sheet can be more conveniently obtained by baking in the drying area of the drying equipment through the transmission of the conveyor belt of the drying equipment.
[0095] Specifically, the predetermined baking time is 20 seconds to 40 seconds. It can be understood that by baking the dipped pole piece in the drying area for 20 seconds to 40 seconds, the glue attached to the surface of the dipped pole piece can be dried quickly while avoiding damage to the dipped pole piece during the drying process. Among them, the predetermined baking time can be 20 seconds, 30 seconds or 40 seconds, which is not limited here. Those skilled in the art can adjust it according to the drying condition of the glue on the surface of the dipped pole piece.
[0096] S200. In one embodiment, the positive electrode sheet is immersed in glue to obtain the dipped electrode sheet, and the method further comprises:
[0097] Step A: Mix the glue liquid and pure water in a predetermined ratio to obtain the glue liquid, wherein the glue liquid can be 48% SBR (styrene butadiene rubber) glue liquid, which is of course not limited here, and those skilled in the art can also replace it as needed.
[0098] In this embodiment, the glue is obtained by mixing the glue liquid with pure water in a predetermined ratio, thereby diluting the glue liquid to avoid excessive concentration of the glue liquid in the glue, thereby ensuring that the positive electrode sheet can be smoothly taken out and enter the next process after being immersed in the glue.
[0099] Specifically, the predetermined ratio of the glue solution to the pure water is 1:10. It can be understood that by keeping the ratio of the glue solution to the pure water at 1:10, it is possible to avoid the glue solution having too high a water content after dilution to be difficult to adsorb and wrap the outer surface of the positive electrode sheet, and it is also possible to avoid the glue solution having too little water content after dilution to be difficult to remove from the glue. Wherein, 1:10 is the weight ratio of the glue solution to the pure water.
[0100] Furthermore, the temperature of the drying zone is 100°C to 125°C. It can be understood that, because 100°C is the boiling point of water, when the dipped electrode enters the drying zone, the moisture in the glue on the dipped electrode can evaporate, thereby allowing the glue on the dipped electrode to dry quickly, and by keeping the temperature of the drying zone below 125°C, the glue on the dipped electrode can be prevented from overheating and being damaged. Among them, the temperature of the drying zone can be set to 100°C, 115°C or 125°C, of course, it is not limited here, and those skilled in the art can adjust it according to the drying rate of the glue on the dipped electrode.
[0101] In one embodiment, before placing the drying electrode pieces in a packing box to collect the drying electrode pieces, the method further includes:
[0102] Step B: placing the drying electrode on a work surface;
[0103] Step C: stacking the drying electrodes to arrange the drying electrodes into groups.
[0104] In this embodiment, before the drying electrode is placed in the packaging box, the drying electrode is placed on a work surface, so that it is more convenient for the operator to stack a plurality of the drying electrode. The stacked drying electrode is organized into groups and can be placed in the packaging box in an orderly manner, which is more convenient for transportation. Specifically, the surface of the drying electrode can be placed perpendicular to the bottom of the packaging box, or the surface of the electrode can be placed parallel to the bottom of the packaging box.
[0105] In one embodiment, before step B: placing the drying electrode on a work surface, the method further includes:
[0106] Step B1: Place the soft silicone pad on the work surface. It is understood that by placing the soft silicone pad on the work surface, the soft silicone pad is soft in texture and can play a certain buffering role during the placement of the drying electrode, thereby effectively preventing the drying electrode from breaking, warping or burring during the placement process.
[0107] In one embodiment, step C: stacking the drying electrodes to arrange the drying electrodes into groups further comprises:
[0108] Step C1: placing a knife card between two adjacent groups of drying electrodes to separate the two adjacent groups of drying electrodes.
[0109] It can be understood that by placing the knife card between two adjacent groups of the drying electrodes, the two adjacent groups of the drying electrodes can be effectively separated to prevent the two adjacent groups of the drying electrodes from rubbing against each other after the drying electrodes are placed in the packaging box, thereby causing the glue on the surface of the drying electrodes to be scratched off. If the glue on the surface of the drying electrodes is scratched off, the wrapping of the glue on the drying electrodes will become worse, thereby aggravating the powdering of the positive electrode.
[0110] In one embodiment, after S400, placing the drying electrode pieces in a packing box to collect the drying electrode pieces, the method further includes:
[0111] S500: Put a label in the packaging box.
[0112] In this embodiment, after the drying electrode sheets are placed in a packaging box, a label is placed in the packaging box so that the user can know the product information of each packaging box through the label. The label indicates product information such as the production time and the number of drying electrode sheets in each packaging box.
[0113] In one embodiment, after S500, placing the label in the packaging box, the method further includes:
[0114] S600, putting the protective cover on the label. It can be understood that by putting the protective cover on the label, the label is protected by the protective cover, so as to avoid the product information on the label being worn during the transportation of the packaging box and affecting subsequent identification.
[0115] Compared with the prior art, the present invention has at least the following advantages:
[0116] The above-mentioned nickel-hydrogen battery positive electrode plate anti-powdering pretreatment method, by immersing the positive electrode plate in the glue, can make the glue adhere to the positive electrode plate, so that the surface of the positive electrode plate can be wrapped by the glue to obtain the dipped electrode plate, and then the dipped electrode plate is placed in the drying equipment, and the dipped electrode plate is baked by the drying equipment to obtain a dried electrode plate, and finally the dried electrode plate is placed in a packing box to collect the dried electrode plate. The dipped electrode plate is baked by the drying equipment so that the glue on the surface of the positive electrode plate is dried to form a film, and the surface of the positive electrode plate becomes more flexible after being wrapped by the glue, and is less likely to crack during softening, cutting edges and winding processes, thereby reducing the occurrence of powdering of the conductive coating on the surface of the positive electrode plate. At the same time, since the surface of the positive electrode plate is wrapped with the glue, the conductive coating is not easy to fall off from the surface of the positive electrode plate after powdering, thereby ensuring that the battery remains in a good state.
[0117] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the patent of the present disclosure shall be subject to the attached claims.
Claims
1. A method for pretreating a nickel-hydrogen battery positive electrode sheet to prevent powder loss, characterized in that: include: Get the positive electrode; Soaking the positive electrode sheet in glue to obtain a glue-impregnated electrode sheet; Placing the dipped electrode in a drying device to obtain a dried electrode; The drying electrode sheets are placed in a packing box to collect the drying electrode sheets.
2. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 1, characterized in that: The positive electrode sheet is immersed in glue to obtain a glue-impregnated electrode sheet, comprising: Placing the positive electrode sheet on a conveyor belt of an automatic glue dipping machine to convey the positive electrode sheet to a glue dipping area of the automatic glue dipping machine; The positive electrode sheet is soaked for a predetermined soaking time to obtain the resin-impregnated electrode sheet.
3. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 2, characterized in that: The predetermined soaking time is 2 seconds to 5 seconds.
4. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 1, characterized in that: Placing the dipped electrode in a drying device to obtain a dried electrode comprises: Placing the dipped electrode on the conveyor belt of the drying equipment to convey the dipped electrode to the drying area of the drying equipment; The dipped electrode is dried for a predetermined baking time to obtain the dried electrode.
5. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 4, characterized in that: The predetermined baking time is 20 seconds to 40 seconds.
6. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 4, characterized in that: The temperature of the drying zone is 100°C to 125°C.
7. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 1, characterized in that: The positive electrode sheet is immersed in glue to obtain the dipped electrode sheet, and the following steps are also included: The glue solution is mixed with pure water in a predetermined ratio to obtain the glue.
8. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 7, characterized in that: The predetermined ratio of the glue solution to the pure water is 1:
10.
9. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 1, characterized in that: Placing the drying electrode sheet in a packing box to collect the drying electrode sheet also includes: Placing the drying electrode on a work surface; The drying electrodes are stacked to arrange the drying electrodes into groups.
10. The method for pretreating nickel-hydrogen battery positive electrode sheets to prevent powder loss according to claim 1, characterized in that: Placing the drying electrode pieces in a packing box to collect the drying electrode pieces further comprises: Place the label in the packaging box.