Lithium ion battery electrode composition and preparation method thereof
By using a combination of carbon molten metal and heteroatom-doped multi-walled carbon nanotubes with active materials, carbon black and polymer binders in lithium-ion battery electrodes, the problem of insufficient electrode conductivity is solved, increasing capacity and life, and enhances battery safety to avoid thermal runaway.
Patent Information
- Application Number
- CN202410443282.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-18
AI Technical Summary
The low conductivity of conductive carbon in existing lithium-ion battery electrodes leads to high rate capacity and cycle life problems, and is insufficient in safety and prone to thermal runaway.
Using carbon-fused metal and heteroatom-doped multi-walled carbon nanotubes (MWCNTs) combined with active materials, carbon black and polymer binders to prepare high interfacial surface area cathode electrodes, specific process steps improve conductivity and Adhesion, enhancing the stability and safety of the electrode.
It achieves improvements in high-rate capacity and cycle life, while improving the safety of lithium-ion batteries. MWCNTs with high thermal conductivity promote proper heat dissipation and avoid thermal runaway.
Smart Images

Figure CN118800908A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the manufacture of lithium-ion batteries with high rates and methods for preparing electrodes thereof using carbon-fused metals and heteroatom-doped multi-walled carbon nanotubes. More specifically, the present invention relates to cathode electrodes for lithium-ion batteries and methods for preparing the same. The cathode is prepared using active materials, carbon black and homemade carbon-fused metals and heteroatom-doped multi-walled carbon nanotubes (MWCNT). MWCNT is prepared from petroleum refining raw materials. MWCNT is a metal and heteroatom-doped CNT, wherein the metal is a transition metal such as Co, Mn, Fe, Ni, etc., and the heteroatom is nitrogen, sulfur, oxygen, phosphorus, etc. A polymer binder is also used in the composition to prepare the cathode electrode. Background Art
[0002] Carbon with high surface area plays a key role in the performance of batteries. The interfacial surface area between the carbon and the active material generally affects the interparticle internal resistance, rate capacity and other properties of the electrode. Together with the surface area of the carbon, its adhesion property is very critical because it increases the life cycle of the battery without degradation and capacity decay of the active material. Although many efforts have been made to improve the performance of batteries using different types of high surface area carbon materials, there is still a need to develop lithium-ion batteries that will increase rate capacity, power density and high cycle life without loss of capacity.
[0003] MWCNTs have many unique properties derived from their small size, cylindrical graphite structure, and high aspect ratio. Carbon nanotubes have extremely high tensile strength, high modulus, good chemical and environmental stability, and high thermal and electrical conductivity. Carbon nanotubes have many applications, including the preparation of conductive, electromagnetic and high-strength composite materials, energy storage systems, etc. In batteries, MWCNTs can be used as conductive agents in cathode and anode electrodes. MWCNTs can also be used as active anode materials for lithium-ion batteries.
[0004] Carbon-fused metal and heteroatom-doped MWCNTs have higher interfacial surface area, whereby it connects with active materials, which also leads to high stability of lithium-ion batteries and higher conductivity and electrode adhesion properties required for cathode electrodes with high rate capability.
[0005] US20140093769A1 provides nanoelement-based electrode materials for rechargeable batteries. The electrodes are based on carbon nanotube (CNT) scaffolds coated with thin layers of electrochemically active materials in the form of nanoparticles. The use of alternating layers of CNTs and active nanoparticles further increases the power density and rate of the battery.
[0006] US8540902B2 describes a paste based on carbon nanotubes and methods for their preparation and use. The carbon nanotubes are dispersed by grinding; the resulting paste has a Hegman scale greater than 7. The paste can be used as a conductivity enhancer in electronic devices such as batteries, capacitors, electrodes or other devices requiring a highly conductive paste.
[0007] US20070190422A1 relates to energy storage devices. Specifically, the present disclosure relates to a lithium-ion battery having two active electrodes composed of carbon nanotube (CNT) materials, wherein lithium metal powder is dispersed in the CNT material of the anode.
[0008] EP3786110A1 relates to a carbon nanotube dispersion excellent in dispersibility and storage stability of the carbon nanotubes. The present disclosure also relates to a battery electrode mix layer and a lithium ion secondary battery including the carbon nanotube dispersion.
[0009] US8,822,078B2 relates to free-standing carbon nanotube paper comprising purified carbon nanotubes, wherein the purified carbon nanotubes form the free-standing carbon nanotube paper, and carbon particles are embedded and / or present on the surface of the carbon nanotube paper. The present disclosure also relates to lithium-ion batteries, capacitors, supercapacitors, batteries / capacitors and fuel cells comprising the free-standing carbon nanotube paper as electrodes.
[0010] US20050181282A1 discloses a high-performance battery based on carbon nanofibers (CNT-carbon nanotubes), which includes a cell slot filled with electrolyte, a spring coil locked to the cell slot, an anode / cathode substrate installed in the cell slot and having its separation membrane, and positive and negative terminals installed on the outside of the cell cover and respectively connected to the anode / cathode substrate.
[0011] US20090246625A1 generally relates to lithium-ion batteries, and more specifically to lithium-ion batteries based on aligned graphene ribbon anodes, V2O5 graphene ribbon composite cathodes, and ionic liquid electrolytes. Lithium-ion batteries have excellent performance metrics of cell voltage, energy density, and power density.
[0012] US20110256451A1 discloses an electronic device comprising: a carbon nanotube film having a plurality of carbon nanotubes; an inorganic coating on the carbon nanotube film; and a conductive electrode coupled to the carbon nanotube film for conducting current therefrom.
[0013] CN105375009A discloses a stable nitrogen-doped carbon nanotube and iron oxide composite anode material, which is based on nitrogen-doped carbon nanotubes and is characterized in that the outer surface of the nitrogen-doped carbon nanotubes is loaded with iron oxide particles, wherein iron oxide is the main component, and the loading amount of iron oxide accounts for 10-90% of the total mass of the iron oxide particles and the nitrogen-doped carbon nanotubes.
[0014] US2016.0020466A1 relates to a dispersion comprising a dispersion medium, a polymer dispersant and carbon nanotubes dispersed in the dispersion medium.
[0015] US10622631B2 includes an anode active material crystalline carbon, which includes natural graphite, artificial graphite, expandable graphite, graphene, carbon nanotubes or a combination thereof and silicon carbon secondary particles.
[0016] EP 3404747A1 describes compositions and properties for preparing expander-free electrodes for lead-acid batteries. It involves the use of heteroatoms, i.e. nitrogen, sulfur intrinsically embedded carbon nanotubes (H-CNTs) as multifunctional additives for preparing lead-acid battery electrodes to replace expander chemicals, i.e. vanilla dispersants, Dinel fibers, barium sulfate and carbon black.
[0017] Ruan, Boyang, et al. Carbon-encapsulated Sn@N-doped carbon nanotubes as anode materials for application in SIBs. ACS applied materials&interfaces 9.43(2017):37682-37693 discloses carbon-encapsulated Sn@N-doped carbon nanotubes as anode materials for application in sodium ion batteries.
[0018] Due to the low conductivity of the conductive carbon used in the electrodes of lithium-ion batteries, the high rate capacity and cycle life issues of lithium-ion batteries remain a problem. In addition, the safety of lithium-ion batteries remains a challenge. Therefore, there is still time to solve the shortcomings associated with lithium-ion batteries.
[0019] Purpose of the Invention
[0020] The main object of the present invention is to provide a lithium ion battery with a high rate capability.
[0021] Another object of the present invention is to disclose a method for preparing electrodes thereof using carbon molten metal and heteroatom doped multi-walled carbon nanotubes. Summary of the invention
[0022] The present invention as embodied and broadly described herein provides a cathode electrode comprising carbon molten metal and heteroatom doped MWCNTs prepared from refined feed, active material, carbon black and polymer binder. The resulting electrode obtained by the method of the present invention effectively overcomes the high rate capacity and cycle life problems of lithium ion batteries / cells due to the low conductivity of conductive carbon used in lithium ion battery electrodes. The present invention also improves the safety of lithium ion batteries because its use of MWCNTs with high thermal conductivity leads to proper heat dissipation throughout the electrodes, thereby avoiding thermal runaway that is very common in lithium ion batteries.
[0023] The present invention provides a cathode electrode for a lithium ion battery, comprising:
[0024] a) Carbon-fused metal and heteroatom-doped multi-walled carbon nanotubes (MWCNTs);
[0025] b) active materials;
[0026] c) carbon black; and
[0027] d) Polymer binders.
[0028] In one embodiment of the present invention, the cathode active material present in the cathode electrode composition accounts for 85-95% by weight of the composition. The carbon molten metal and heteroatom doped MWCNT present in the cathode electrode composition accounts for 0.5-6% by weight of the composition. Carbon black is present in the range of 0.5-6% by weight of the composition. The polymer binder is present in the range of 1-5% by weight of the composition.
[0029] The present invention also provides a method for preparing a cathode for a lithium ion battery, the method comprising preparing metal and heteroatom doped MWCNTs from refined raw materials, then preparing higher interfacial carbon molten metal and heteroatom doped MWCNTs, further subsequently preparing cathode electrode slurry, and finally preparing a cathode electrode.
[0030] The present invention also provides a method for preparing a cathode electrode for a lithium ion battery, comprising the following steps:
[0031] a). Preparation of metal and heteroatom doped MWCNTs from refined raw materials;
[0032] b) preparing carbon-molten metal- and heteroatom-doped MWCNTs from the metal- and heteroatom-doped MWCNTs obtained above;
[0033] a). Prepare the cathode electrode paste as follows: Mix 85 - 95 wt% of the active material with 0.5 - 6 wt% of the carbon - molten metal and heteroatom - doped MWCNT, then mix with 0.5 - 6 wt% of carbon black to obtain a mixture, and then add 1 - 5 wt% of the polymer binder to the above - mentioned mixture; and
[0034] d). Fabricate the cathode electrode.
[0035] In another aspect, the present invention provides a lithium - ion battery, which comprises:
[0036] a) A cathode electrode made of an active material, carbon - molten metal and heteroatom - doped MWCNT, carbon black and a polymer binder; and
[0037] b) A graphite anode.
[0038] The present invention also provides a new electrode composition for a lithium - ion battery with high rate capacity and high cycle life.
[0039] The carbon - molten metal - doped heteroatom MWCNT has good adhesion properties, which results in a stable life cycle without capacity fade.
[0040] Compared with MWCNT prepared from pure gaseous molecules, the carbon - molten metal - doped heteroatom MWCNT prepared indigenously from crude oil and its products has a lower cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] When read in conjunction with the accompanying drawings, the present invention will be correctly interpreted. Descriptions of the embodiments of the drawings are given here.
[0042] Figure 1 A Raman Shift diagram of the carbon - molten metal and heteroatom - doped MWCNT is shown.
[0043] Figure 2 An XRD diagram of the carbon - molten metal and heteroatom - doped MWCNT is shown.
[0044] Figure 3 A TGA diagram of the carbon - molten metal and heteroatom - doped MWCNT is shown.
[0045] Figure 4 A Cyclic Voltammetry diagram of the LiFePO4 cathode doped with the carbon - molten metal and heteroatom - doped MWCNT is shown.
[0046] Figure 5 A low - resolution TEM image (low magnification) of the carbon - molten metal and heteroatom - doped MWCNT is shown.
[0047] Figure 6 HR-TEM images (high magnification) of carbon-fused metal and heteroatom-doped MWCNTs are shown.
[0048] Figure 7 Shown is a graph comparing the rate capacity of NMC 811 cathode doped with carbon fused metal and heteroatom doped MWCNTs to a control box.
[0049] Figure 8 Shown is a graph comparing the rate capacity of NCA cathodes doped with carbon-fused metal and heteroatom-doped MWCNTs with a control box.
[0050] Fig. 9 Shown is the life cycle comparison of NMC 811 cathode doped with carbon fused metal and heteroatom doped MWCNTs with control box and commercial MWCNTs. DETAILED DESCRIPTION
[0051] First, it should be understood that although illustrative implementations of embodiments of the present disclosure are shown below, the present invention may be implemented using any number of techniques, whether currently known or in existence. The present invention should in no way be limited to the illustrative implementations, drawings, and techniques described below, including the exemplary designs and implementations illustrated and described herein, but may be modified within the scope of the appended claims along with the full scope of their equivalents.
[0052] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0053] The terms and structures used herein are intended to describe, teach, and illustrate some embodiments and specific features and elements thereof, but not to limit, restrict, or narrow the scope of the claims or their equivalents.
[0054] As used herein, a "doctor blade" is a tool that applies a desired thickness of electrode material.
[0055] "Active material" as defined in the present invention is the capacity carrying material of the battery, ie, a lithium-based metal oxide.
[0056] As defined herein, "crude oil related products" or "refinery feedstocks" refer to heavy naphtha, light naphtha, and combinations thereof.
[0057] The "ID / IG" ratio as used in the present invention is used to define defects in a carbon sample. If the ID / IG ratio is larger, there are more defects in the carbon sample, and vice versa.
[0058] The present invention provides a cathode electrode for a lithium ion battery, comprising:
[0059] a) Carbon-fused metal and heteroatom-doped multi-walled carbon nanotubes (MWCNTs);
[0060] b) active materials;
[0061] c) carbon black; and
[0062] d) Polymer binders.
[0063] In one embodiment of the present invention, carbon fused metal and heteroatom doped MWCNTs are present in the range of 0.5-6 wt%.
[0064] In another embodiment of the present invention, the active material is selected from lithium nickel-manganese-cobalt oxide (NMC), lithium nickel-cobalt-aluminum oxide (NCA) and lithium iron phosphate (LFP), lithium nickel manganese spinel (LNMO), lithium manganese oxide (LMO) and lithium cobalt oxide (LCO), and the active material is present in the range of 85-95 weight %.
[0065] In yet another feature of the present invention, carbon black is present in the range of 0.5-6 wt%.
[0066] In yet another feature of the invention, the polymer binder is polyvinylidene fluoride in the range of 1-5 wt%.
[0067] The present invention also provides a method for preparing a cathode electrode for a lithium ion battery, the method comprising the following steps:
[0068] a). Preparation of metal and heteroatom doped MWCNTs from refined raw materials;
[0069] b) preparing carbon-molten metal- and heteroatom-doped MWCNTs from the metal- and heteroatom-doped MWCNTs obtained above;
[0070] c) preparing a cathode electrode slurry by mixing 85-95 wt % of the active material with 0.5-6 wt % of the carbon molten metal and heteroatom doped MWCNT, and then mixing with 0.5-6 wt % of carbon black to obtain a mixture, and then adding 1-5 wt % of a polymer binder to the above mixture; and
[0071] d). Manufacturing cathode electrode.
[0072] In one feature of the invention, step (a) of the method comprises:
[0073] I. using hydrogen to reduce the catalyst in a reactor, the reactor being operated at three different temperature zones of about 620-640° C., 645-665° C., and 670-690° C. and a pressure of about 1 atmosphere;
[0074] II. In the presence of nitrogen carrier gas, the refined feedstock was fed into the reactor at a flow rate of 25-45 ml / h for 10 hours;
[0075] III. Add 0.1-1 g of doped MWCNT and dilute sulfuric acid (50–550 ml) and disperse for 0.5-1 hour to obtain a mixture;
[0076] IV. The mixture of step III is refluxed at 80-100 ° C at a speed of 200-500 rpm for 2-6 hours to obtain a reaction mixture;
[0077] V. adding distilled water to the reaction mixture of step IV and maintaining for 10-15 minutes, then decanting and filtering; and
[0078] VI. After step V was repeated 4-5 times, the obtained mixture was washed to a neutral pH, then dried at 100-120° C. for 8-12 hours and weighed to obtain metal and heteroatom doped MWCNTs.
[0079] In another feature of the present invention, step (b) of the method for preparing a cathode electrode for a lithium ion battery comprises:
[0080] I. grinding 1-20 g of carbon black with 80-99 g of metal and heteroatom doped MWCNTs to obtain a powder;
[0081] II. The powder obtained in step I was ultrasonically treated in NMP solvent for 0.5-1 hour to obtain the resulting mixture;
[0082] III. The resulting mixture is filtered, then dried and calcined to obtain carbon-fused metal and heteroatom doped MWCNTs.
[0083] In another feature of the present invention, step (c) of the method for preparing a cathode electrode for a lithium ion battery comprises:
[0084] I. mixing the carbon molten metal and heteroatom doped MWCNT with the active material and then adding carbon black to obtain the mixture, wherein the active material is selected from the group consisting of NMC, NCA, LFP, LNMO, LMO and LCO and combinations thereof;
[0085] II. Obtain NMP solution containing polymer binder and add to the above mixture and stir for 2-8 hours to obtain a uniform cathode electrode slurry.
[0086] In another feature of the present invention, step (d) of the method for preparing a cathode electrode for a lithium ion battery comprises:
[0087] I. coating the cathode electrode slurry on an aluminum foil with a coating thickness of 100-300 mm; and
[0088] II. The cathode electrode of step I is placed in a vacuum oven at 100-120° C. and dried overnight to obtain the cathode for lithium-ion batteries.
[0089] In yet another feature of the present invention, the metal and heteroatom doped MWCNTs contain Co: 0.01-3100 ppm, Mn: 0.01-800 ppm, Fe: 0.01-400 ppm, S: 0.001-1 wt% and N: 0.01-2000 ppm.
[0090] The present invention also provides a lithium ion battery, comprising:
[0091] a) cathode electrode made of active material, carbon fused metal and heteroatom doped MWCNT, carbon black and polymer binder; and
[0092] b) Graphite anode.
[0093] In one feature of the invention, the lithium-ion battery outputs a capacity of up to 5C rate, and the cell outputs 80-100 mAhg at 1C rate. -1 The specific capacity of the battery is 2.75-4.2V, and the battery cell shows excellent cycling stability when cycled between 2.75-4.2V.
[0094] The present disclosure relates to the manufacture of lithium-ion batteries with high rates and methods for preparing electrodes thereof using carbon-molten metal and heteroatom doped multi-walled carbon nanotubes. The cathode is prepared with active materials, carbon black and homemade carbon-molten doped MWCNTs. MWCNTs are prepared from petroleum refining raw materials. MWCNTs are metal and heteroatom doped CNTs, wherein the metal is a transition metal such as Co, Mn, Fe, Ni, etc., and the heteroatom is nitrogen, sulfur, oxygen, phosphorus, etc. A polymer binder is also used in the composition to prepare the cathode electrode.
[0095] In one embodiment, the present invention discloses a method and composition for preparing a lithium ion battery cell electrode. The cathode active material present in the cathode electrode composition accounts for 85-95% by weight of the composition. The carbon molten metal and heteroatom doped MWCNT present in the cathode electrode composition account for 0.5-6% by weight of the composition. Carbon black is present in the range of 0.5-6% by weight of the composition. The polymer binder is present in the range of 1-5% by weight of the composition.
[0096] The refined raw materials in the present invention include low-sulfur crude oil, high-sulfur crude oil and mixtures thereof.
[0097] In one of the other embodiments, the present invention comprises the following method for preparing a cathode electrode comprising the steps of:
[0098] 1). Preparation of metal and heteroatom doped MWCNTs from refined raw materials, including:
[0099] 1a). Hydrogen is used to reduce the catalyst in the reactor. Thereafter, crude oil related products are fed into the reactor. The reactor is operated in three temperature zones maintained at about 630°C, 655°C and 680°C. The reactor is operated at a pressure of about 1 atmosphere. The catalyst used in the process is an Fe-Co catalyst or a Fe-Mo catalyst supported on alumina.
[0100] Metal- and heteroatom-doped MWCNTs with 15-40 layers or more and an outer diameter (OD) of 20-40 nm and an inner diameter (ID) of 5-17 nm can be prepared from refined raw materials by the following method:
[0101] 8g of alumina-supported catalyst was loaded into the middle of a vibrating reactor. The flow rate of the carrier and the reducing gas was controlled by an electronic mass flowmeter, and the temperature of the catalyst and the reactor was measured by a thermocouple. In the presence of a nitrogen carrier gas, the catalyst was further heated to 700°C. After reaching the desired temperature of 700°C, hydrogen (75sccm) was introduced into the reactor to reduce the catalyst and continue to reduce for 4 hours. After the catalyst reduction was completed, the reactor temperature was reduced to 600°C in a nitrogen atmosphere. At this stage, high-sulfur crude oil with a sulfur content of>1% by weight was fed into the reactor with a flow rate of 14g / h and a nitrogen carrier gas of 50sccm and continued for 430min. The product gas stream was further analyzed by a refinery gas analyzer. The chromatogram shows the production pattern of gases (such as hydrogen, nitrogen, methane and other light hydrocarbons). After the operation was completed, the reactor was cooled in a nitrogen atmosphere and solid carbon nanotubes were collected and the yield was estimated.
[0102] 1b). The required amount of doped MWCNTs (0.1-1 grams) prepared by the above method and dilute sulfuric acid (50-550 ml) were added to a round bottom glass flask and the MWCNTs were dispersed in an ultrasonic bath for 0.5-1 hour. Thereafter, the same mixture was refluxed on a hot plate at 80-100°C at a speed of 200-500 rpm for 2-6 hours. Then, distilled water was added to the same flask and kept as it was for 10-15 minutes, which was then decanted, and the sample was then filtered on a membrane filter and repeated 4-5 times. Afterwards, it was washed to neutral pH, dried at 100-120°C for 8-12 hours and weighed to obtain the desired metal and heteroatom doped MWCNTs. (Co: 0.01-3100ppm, Mn: 0.01-800ppm, Fe: 0.01-400ppm, S: 0.001-1 wt% and N: 0.01-2000ppm).
[0103] 2). Preparation of higher interfacial carbon fused metal and heteroatom doped MWCNTs:
[0104] 2a). 10 g of carbon black was milled with 90 g of metal and hetero-doped MWCNTs in an ethanol solvent at 500 rpm at room temperature in a planetary ball mill for 1-4 hours.
[0105] 2b). The resulting mixture was filtered and then kept in a vacuum oven at 200°C for 6-10 hours.
[0106] 2c). The powder is kept in a furnace at 1000-1400°C in an inert atmosphere. The heating rate is 200°C / hour until a temperature of 1000-1400°C is reached, and then the same temperature is maintained for 2-4 hours, followed by natural cooling to room temperature.
[0107] 2d). During the whole process, the flow rate of argon was maintained at 100 ml / h.
[0108] 3). Preparation of cathode electrode slurry:
[0109] 3a). Cathode active material (NMC / NCA / LFP, LNMO, LCO and LMO etc.) accounts for 85-95 wt% of the composition and is mixed with 0.5-6 wt% of carbon molten metal and heteroatom doped MWCNT by means of mortar pestle / vacuum mixer for 15 minutes to 1 hour. The resulting powder mixture is then further mixed with 0.5-6 wt% of carbon black and ground for 15 minutes to 1 hour.
[0110] 3b). A solution of a polymer binder polyvinylidene fluoride (PVDF) in NMP (N-methyl-2-pyrrolidone) accounting for 1-5 wt% of the total composition is added to the above solution and stirred on a magnetic stirrer for 2-8 hours to obtain a uniform slurry.
[0111] 4). Manufacturing of cathode electrode:
[0112] 4a). The cathode slurry prepared as above was coated on an aluminum foil with a doctor blade applicator at an application thickness of 100-300 mm. The cathode electrode was then placed in a vacuum oven at 100-120° C. to dry overnight.
[0113] In one of more embodiments, the present invention discloses the use of low-grade carbon black, which is a very cheap conductive material available in the market, together with metal-doped heteroatom MWCNTs for lithium-ion battery applications.
[0114] In another embodiment, the present invention discloses the use of carbon molten metal and heteroatom-doped MWCNTs with ID / IG: 0.740±0.1, 30-40 layers, and carbon black in electrodes to manufacture lithium-ion full cells with high rate capacity.
[0115] In another further embodiment, the present invention discloses using carbon molten metal and a BET surface area of 120±10 m 2 / gram of heteroatom-doped MWCNTs and carbon black to manufacture lithium-ion full-cells with high rate capacity.
[0116] In one or more embodiments, the present invention discloses the use of highly purified carbon fused metal and heteroatom doped MWCNTs (confirmed by TGA) and carbon black in electrodes to prepare lithium ion full cells with high rate capacity.
[0117] In another further embodiment, the present invention discloses the use of highly graphitic carbon fused metal and heteroatom doped MWCNTs (confirmed by XRD) and carbon black in electrodes to fabricate lithium ion full cells with high rate capacity.
[0118] According to one aspect of the subject matter, in the described embodiments, the carbon-coated metal-doped heteroatom MWCNTs have a higher interfacial surface area (confirmed by CV electrochemical studies), whereby it connects the active materials, which also leads to high stability of lithium-ion batteries and higher conductivity and electrode adhesion properties required for cathode electrodes with high rates.
[0119] In yet another embodiment, the present invention provides for the formation of a lithium ion battery having high Coulombic efficiency.
[0120] According to one aspect of the subject matter, in the described embodiments, the optimized composition of carbon-fused metal and heteroatom-doped MWCNTs in the cathode electrode avoids irreversible capacity loss.
[0121] In a preferred embodiment, the present invention discloses the manufacture of lithium-ion all-button cells with high power density and high rate capacity.
[0122] In another more preferred embodiment, the present invention discloses the preparation of cathodes using carbon molten MWCNTs prepared from petroleum refining feedstocks. MWCNTs are CNTs doped with metals and heteroatoms, wherein the metals are heavy metals such as Co, Mn, Fe, Ni, etc., and the heteroatoms are nitrogen, oxygen, sulfur, phosphorus, etc.
[0123] In a further preferred embodiment, the present invention discloses that the full cell of the 2032 button cell manufactured by using the above-mentioned material can output the capacity of up to 5C rate at a high rate, and output 80-100 mAhg at 1C rate. -1 , and exhibits excellent cycling stability when cycled between 2.75–4.2 V.
[0124] Advantages and improvements of the present invention over existing methods:
[0125] 1. Carbon fused metal and heteroatom doped MWCNTs prepared from petroleum refinery feedstocks can be used with low quality cheap carbon blacks that are not suitable for lithium ion battery applications.
[0126] 2. Carbon-fused metal and heteroatom-doped MWCNT particles are compatible with low-quality carbon black and also lead to higher interfacial interactions between their particles and active material particles.
[0127] 3. This interaction also helps to enhance the adhesion properties of the active materials, which results in a stable cathode with high rate and high life cycle.
[0128] Example
[0129] The invention will now be illustrated by means of non-limiting examples.
[0130] Example 1: Preparation of desired metal and heteroatom-doped MWCNTs from refined raw materials
[0131] Hydrogen is used to reduce the catalyst in the reactor. The reactor is operated in three temperature zones maintained at about 630°C, 655°C and 680°C. The reactor is operated under a pressure of about 1 atmosphere. Crude oil related products are fed to the reactor at a flow rate of 35 ml / hour for 10 hours in the presence of a nitrogen carrier gas to obtain metal and heteroatom doped MWCNT. About 0.1-1 grams of doped MWCNT and dilute sulfuric acid (50-550ml) produced are added to a round bottom glass flask, and the MWCNT is dispersed in an ultrasonic bath for 0.5-1 hour. Thereafter, the same mixture is refluxed on a hot plate at 80-100°C with a speed of 200-500rpm. Then, distilled water was added to the same flask and kept for 10-15 minutes, then it was decanted and the sample was filtered on a membrane filter, and this was repeated 4-5 times, then washed to neutral pH, dried at 100-120°C for 8-12 hours, and weighed to obtain the desired metal and heteroatom doped MWCNTs (Co: 0.01-3100 ppm, Mn: 0.01-800 ppm, Fe: 0.01-400 ppm, S: 0.001-1 wt% and N: 0.01-200 ppm).
[0132] Example 2: Preparation of higher interfacial carbon-fused metal and heteroatom-doped MWCNTs:
[0133] 1. 10 g of carbon black and 90 g of metal- and heteroatom-doped MWCNTs were ground together in a planetary ball mill at 500 rpm at room temperature for 1-3 hours, and then the resulting powder was sonicated in NMP solvent for 0.5-1 hour.
[0134] 2. Filter the resulting mixture and then keep it in a vacuum oven at 200°C for 6-10 hours.
[0135] 3. The powder is kept in a furnace at 1000-1400°C in an inert atmosphere. The heating rate is 200°C / hour until a temperature of 1000-1400°C is reached, and then the same temperature is maintained for 2-4 hours, followed by natural cooling to room temperature.
[0136] 4. During the whole process, the flow rate of argon was maintained at 100 ml / h.
[0137] Example 3: Preparation of NMC 811 cathode electrode
[0138] Take 1.8 grams of cathode active material NMC 811 (lithium nickel-manganese-cobalt oxide) and mix with 68 mg of carbon molten metal and heteroatom doped MWCNT by mortar pestle / vacuum mixer for 15 minutes-1 hour, then add 24 mg of carbon black and grind for 15 minutes-2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 52 mg of total composition weight to the above solution and stir it on a magnetic stirrer for 2-8 hours to obtain a uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0139] Example 4: Preparation of NMC 811 cathode electrode
[0140] Take 1.8 grams of cathode active material NMC 811 (lithium nickel-manganese-cobalt oxide) and mix with 88 mg of carbon molten metal and heteroatom doped MWCNT by mortar pestle / vacuum mixer for 15 minutes-1 hour, then add 32 mg of carbon black and grind for 15 minutes-2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of total composition weight to the above solution and stir it on a magnetic stirrer for 2-8 hours to obtain a uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0141] Example 5: Preparation of NCA cathode electrode
[0142] Take 1.8 grams of cathode active material NCA (lithium nickel-cobalt aluminum oxide) and mix with 68 mg of carbon molten metal and heteroatom doped MWCNT with the aid of a mortar pestle / vacuum mixer for 15 minutes to 1 hour, then add 24 mg of carbon black and grind for 15 minutes to 2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of the total composition weight to the above solution and stir it under a magnetic stirrer for 2-8 hours to obtain a uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0143] Example 6: Preparation of NCA cathode electrode
[0144] Take 1.8 grams of cathode active material NCA (lithium nickel-cobalt aluminum oxide) and mix with 88 mg of carbon molten metal and heteroatom doped MWCNT with the aid of a mortar pestle / vacuum mixer for 15 minutes to 1 hour, then add 32 mg of carbon black and grind for 15 minutes to 2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of the total composition weight to the above solution and stir it under a magnetic stirrer for 2-8 hours to obtain a uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0145] Example 7: Preparation of LiFePO4 cathode electrode
[0146] Take 1.8 grams of cathode active material LiFePO4 electrode (lithium iron phosphate) (LFP) and mix with 68 mg of carbon molten metal and heteroatom doped CNT by mortar and pestle / vacuum mixer for 15 minutes-1 hour, then add 24 mg of carbon black and grind for 15 minutes-2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of total composition weight to the above solution and stir it under magnetic stirrer for 2-8 hours to obtain a uniform uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0147] Example 8: Preparation of LiFePO4 cathode electrode
[0148] Take 1.8 grams of cathode active material LiFePO4 electrode (lithium iron phosphate) (LFP) and mix with 88 mg of carbon molten metal and heteroatom doped MWCNT with the aid of mortar pestle / vacuum mixer for 15 minutes-1 hour, then add 32 mg of carbon black and grind for 15 minutes-2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of total composition weight to the above solution and stir it on a magnetic stirrer for 2-8 hours to obtain a uniform homogeneous slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0149] Example 9: Fabrication / Testing of Li-ion 2032 Coin Cell Using Carbon Molten Metal and Heteroatom-doped MWCNT-based NMC 811 Cathode
[0150] 9a). Preparation of cathode electrode
[0151] Take 1.8 grams of cathode active material NMC 811 (lithium nickel-manganese-cobalt oxide) and mix with 48 mg of carbon molten metal and heteroatom doped MWCNT by mortar pestle / vacuum mixer for 15 minutes-1 hour, then add 70 mg of carbon black and grind for 15 minutes-2 hours. Then add 2.7 ml of NMP solution of polymer binder accounting for 82 mg of total composition weight to the above solution and stir it on a magnetic stirrer for 2-8 hours to obtain a uniform slurry. Then cut the cathode electrode into 16 mm diameter discs.
[0152] 9b). Preparation of anode electrode
[0153] Take 85-90 wt% of the anode active material graphite and mix it with 6 wt% of the carbon black with the help of mortar pestle / vacuum mixer for 15 minutes to 1 hour. Add 1-5 wt% of the polymer binder in NMP to the above solution and stir it on a magnetic stirrer overnight to get a uniform slurry. Then cut the anode electrode into 16 mm diameter discs.
[0154] 9c). Manufacturing of lithium-ion 2032 button cell
[0155] CR2032 coin cells were assembled in an argon-filled glove box using a graphite electrode as anode, an NMC 811 cathode electrode (prepared as above), a polypropylene celgard polymer separator, and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different ratios of EC / EMC / DMC organic solvents with an additive of ethylene carbonate (VC). The coin cells were cycled between 2.75V and 4.2V on a biologicBCS 805 battery cycler. The fabricated 2032 coin cells were tested at various rates for rate capacity studies.
[0156]
[0157] Doped MWCNTs prepared from refined raw materials exhibit high rate capacity in lithium-ion 2032 full coin cells.
[0158] Example 10: Comparison of life cycle of doped MWCNTs, commercial MWCNTs and control boxes in lithium-ion full cells
[0159] Anode and cathode electrodes were prepared in a manner similar to that in Example 1. CR2032 button cells were assembled in an argon-filled glove box using a graphite electrode (prepared as above) as the anode, a polypropylene celgard polymer separator, and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different proportions of EC / EMC / DMC organic solvents and an additive of vinylene carbonate (VC). The button cells were cycled between 2.75V and 4.2V on a biologic BCS 805 battery cycler. The manufactured 2032 button cells were tested for life cycle studies. The capacity of the manufactured full battery observed at a 1C rate during the cycle is given below.
[0160]
[0161] Example 11: Comparison of Capacity Retention of Novel Doped MWCNTs, Control Boxes, and Commercially Available MWCNTs in Lithium-Ion Cells
[0162] Anode and cathode electrodes were prepared in a manner similar to that in Example 1. CR2032 button cells were assembled in an argon-filled glove box using a graphite electrode (prepared as above) as the anode, a polypropylene celgard polymer separator, and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different proportions of EC / EMC / DMC organic solvents and an additive of ethylene carbonate (VC). The button cells were cycled between 2.75V and 4.2V on a biologic BCS 805 battery cycler. The manufactured 2032 button cells were tested for life cycle studies. The total retention capacity of the manufactured full cell observed at a 1C rate during cycling is given below.
[0163]
[0164] Example 12: Rate Capacity of NCA Cathode Electrode and Comparison with Control Box
[0165] The cathode active material NCA (lithium nickel-cobalt-aluminum oxide) accounted for 85-95 wt% of the composition and was mixed with 60-100 mg of carbon molten metal and heteroatom doped MWCNTs by means of a mortar pestle / vacuum mixer for 15 minutes-1 hour. Then, a NMP solution of a polymer binder accounting for 1-5 wt% of the total composition was added to the above solution and stirred overnight under a magnetic stirrer to obtain a uniform homogeneous slurry. The cathode electrode was then cut into 16 mm diameter discs. CR2032 semi-button cells were assembled in an argon-filled glove box using lithium foil as anode, polypropylene celgard polymer separator and an electrolyte consisting of 1M lithium hexafluorophosphate in different ratios of EC / EMC organic solvents and additive ethylene carbonate (VC). The button cells were cycled between 2.75V and 4.2V on a biologic BCS 805 battery cycler. The manufactured 2032 semi-button cells were tested at various rates for rate capacity studies.
[0166]
[0167] Doped MWCNTs prepared from refined raw materials exhibit high rate capacity in lithium-ion 2032 half-coin cells.
[0168] Example 13: Fabrication / Testing of Li-ion 2032 All-Button Cells Using Carbon-Melted Metal and Heteroatom-Doped MWCNTs
[0169] 13a). Preparation of cathode electrode
[0170] The cathode active material NCA (lithium nickel-cobalt aluminum oxide) accounts for 85-95% by weight of the composition and is mixed with 0.5-6% by weight of carbon molten metal and heteroatom-doped MWCNT by means of a mortar pestle / vacuum mixer for 15 minutes to 1 hour, then 0.5-6% by weight of carbon black is added and ground for 15 minutes to 2 hours. Then a NMP solution of a polymer binder accounting for 1-5% by weight of the total composition is added to the above solution and stirred overnight on a magnetic stirrer to obtain a uniform slurry. The cathode electrode is then cut into 16 mm diameter discs.
[0171] 13b). Preparation of anode electrode
[0172] Take 85-90 wt% of the anode active material graphite and mix it with 6 wt% of the carbon black with the help of mortar pestle / vacuum mixer for 15 minutes to 1 hour. Add 1-5 wt% of the polymer binder in NMP to the above solution and stir it overnight under a magnetic stirrer to get a uniform slurry. Then cut the anode electrode into 16 mm diameter discs.
[0173] 13c). Manufacturing of lithium-ion 2032 full button cell:
[0174] CR2032 all-button cells were assembled in an argon-filled glove box using a graphite electrode as anode, an NMC 811 cathode electrode (prepared as above), a polypropylene celgard polymer separator, and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different ratios of EC / EMC / DMC organic solvents with an additive of ethylene carbonate (VC). The coin cells were cycled between 2.75V and 4.2V on a biologicBCS 805 battery cycler. The fabricated 2032 all-button cells were tested at various rates for rate capacity studies.
[0175]
[0176] Example 14: Higher conductivity of carbon melt-doped MWCNT LiFePO4 cathode (lithium iron phosphate) and its comparison with control box
[0177] The cathode slurry is prepared by using LiFePO4 (lithium iron phosphate) active cathode material accounting for 85-95% by weight of the total composition, and then mixing with 0.5-6% by weight of carbon molten metal and heteroatom doped MWCNT, 0.5-6% by weight of carbon black. Then, the cathode slurry is prepared using an NMP solution of a polymer binder accounting for 1-5% by weight of the total composition. Prior to the slurry preparation, the carbon black is dispersed in NMP for 10 minutes to 0.5 hours with a rest interval of 2-5 minutes. The cathode electrode is then cut into discs of 16 mm diameter. A cathode working electrode area of 1.77 cm is used. 2 CR2032 button cells with different compositions of pure metals and heteroatom-doped MWCNTs were assembled in an argon-filled glove box using lithium foil as the counter electrode, celgard polymer separator and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different proportions of ethylene carbonate / diethylene carbonate organic solvents. -1 Cyclic voltammetry (CV) tests were performed at a scan rate of 1.3 Å. The anodic / cathodic peak currents (mA / g) observed from MWCNTs doped with different percentages of pure metals and heteroatoms are given below.
[0178]
[0179] The CV curves of the carbon melt-doped MWCNT-LFP electrode showed higher anodic and cathodic peak currents compared to the control electrode. The potential interval between the two redox peaks of the LFP-MWCNT electrode was smaller than that of the control electrode, reflecting its small polarization, high ion diffusion, and low internal resistance. The excellent conductivity of carbon melt-doped MWCNT facilitates electron transfer and reduces resistance during the reversible reaction of lithium ions.
[0180] Example 15: Higher interfacial area and conductivity of carbon melt-doped MWCNT LiFePO4 (LFP) cathode (lithium iron phosphate) and its comparison with control box
[0181] The cathode slurry is prepared by using LiFePO4 (lithium iron phosphate) active cathode material accounting for 85-95% by weight of the total composition, and then mixing with 0.5-6% by weight of carbon molten metal and heteroatom doped MWCNT, 0.5-6% by weight of carbon black. Then, the cathode slurry is prepared using an NMP solution of a polymer binder accounting for 1-5% by weight of the total composition. Prior to the slurry preparation, the carbon black is dispersed in NMP for 10 minutes to 0.5 hours with a rest interval of 2-5 minutes. The cathode electrode is then cut into discs of 16 mm diameter. A cathode working electrode area of 1.77 cm is used. 2CR2032 button cells with different compositions of pure metals and heteroatom-doped MWCNTs were assembled in an argon-filled glove box using lithium foil as the counter electrode, celgard polymer separator and an electrolyte consisting of 1-1.22M lithium hexafluorophosphate in different ratios of ethylene carbonate / diethyl carbonate organic solvent. -1 Cyclic voltammetry (CV) tests were performed at a scan rate of 1.3 Å. The anodic / cathodic peak currents (mA / g) observed from MWCNTs doped with different percentages of pure metals and heteroatoms are given below.
[0182]
[0183] The anodic and cathodic peaks appear at about 3.6 V and about 3.2 V, which correspond to the Fe 2+ / Fe 3+ The peak separation between oxidation and reduction of the redox couple in the melt-doped cathode electrode is 72 mV lower than that in the control box, indicating that the carbon in the melt-doped cathode covers all the LFP cathode particles with high interfacial area and produces efficient electron conduction during the electrochemical reaction.
Claims
1. A cathode electrode for a lithium ion battery, comprising: a) Carbon-fused metal and heteroatom-doped multi-walled carbon nanotubes (MWCNTs); b) active materials; c) carbon black; and d) Polymer binders.
2. The electrode according to claim 1, wherein the carbon fused metal and heteroatom doped MWCNTs are present in an amount ranging from 0.5 to 6 wt%.
3. The electrode according to claim 1, wherein the active material is selected from lithium nickel-manganese-cobalt oxide (NMC), lithium nickel-cobalt-aluminum oxide (NCA) and lithium iron phosphate (LFP), lithium nickel manganese spinel (LNMO), lithium manganese oxide (LMO) and lithium cobalt oxide (LCO), and the active material is present in an amount ranging from 85-95 weight %.
4. The electrode according to claim 1, wherein the carbon black is present in an amount ranging from 0.5 to 6 wt%.
5. The electrode according to claim 1, wherein the polymer binder is polyvinylidene fluoride in the range of 1-5 wt%.
6. A method for preparing a cathode electrode for a lithium ion battery, the method The following steps are involved: a). Preparation of metal and heteroatom doped MWCNTs from refined raw materials; b) preparing carbon-molten metal- and heteroatom-doped MWCNTs from the metal- and heteroatom-doped MWCNTs obtained above; c) preparing a cathode electrode slurry by mixing 85-95 wt % of the active material with 0.5-6 wt % of carbon molten metal and heteroatom doped MWCNTs, and then mixing with 0.5-6 wt % of carbon black to obtain a mixture, and then adding 1-5 wt % of a polymer binder to the above mixture; as well as d). Manufacturing cathode electrode.
7. The method according to claim 6, wherein step (a) include: I. using hydrogen to reduce the catalyst in a reactor, the reactor being operated at three different temperature zones of about 620°C-640°C, 645°C-665°C and 670°C-690°C and a pressure of about 1 atmosphere; II. In the presence of nitrogen carrier gas, the refined feedstock is fed into the reactor at a flow rate of 25-45 ml / h for 10 hours; III. Add 0.1-1 g of doped MWCNT and dilute sulfuric acid (50–550 ml) and disperse for 0.5-1 hour to obtain a mixture; IV. The mixture of step III is refluxed at 80 ℃-100 ℃ at a speed of 200-500 rpm for 2-6 hours to obtain a reaction mixture; V. adding distilled water to the reaction mixture of step IV and maintaining for 10-15 minutes, then decanting and filtering; and VI. After step V was repeated 4-5 times, the obtained mixture was washed to a neutral pH, then dried at 100° C.-120° C. for 8-12 hours and weighed to obtain metal and heteroatom doped MWCNTs.
8. The method according to claim 6, wherein said step (b) include: I. grinding 1-20 g of carbon black with 80-99 g of metal and heteroatom doped MWCNTs to obtain a powder; II. The powder obtained in step I is ultrasonically treated in NMP solvent for 0.5-1 hour to obtain the resulting mixture; and III. The resulting mixture is filtered, then dried and calcined to obtain carbon-fused metal and heteroatom doped MWCNTs.
9. The method according to claim 6, wherein said step (c) include: I. mixing the carbon molten metal and heteroatom doped MWCNT with the active material and then adding carbon black to obtain the mixture, wherein the active material is selected from the group consisting of NMC, NCA, LFP, LNMO, LMO and LCO and combinations thereof; as well as II. Obtain NMP solution containing polymer binder and add to the above mixture and stir for 2-8 hours to obtain a uniform cathode electrode slurry.
10. The method according to claim 6, wherein said step (d) include: I. coating the cathode electrode slurry on an aluminum foil with a coating thickness of 100-300 mm; as well as II. The cathode electrode of step I is placed in a vacuum oven at 100-120° C. and dried overnight to obtain the cathode for lithium-ion batteries.
11. The method of claim 7, wherein the metal and heteroatom doped MWCNTs comprise: Co: 0.01-3100 ppm, Mn: 0.01-800 ppm, Fe: 0.01-400 ppm, S: 0.001-1 wt% and N: 0.01-2000 ppm.
12. A lithium ion battery comprising: a) a cathode electrode according to claim 1 or obtained by the method according to claims 6-11; and b) Graphite anode.
13. The lithium ion battery according to claim 12, wherein the battery outputs a capacity of up to 5C rate, and the battery outputs 80-100 mAhg at 1C rate. -1 The battery has a specific capacity of , and exhibits excellent cycle stability when cycled between 2.75-4.2V.
Citation Information
Patent Citations
Stable nitrogen-doped carbon nanotube and iron oxide composite anode material and preparation method thereof
CN105375009A
Compositions for preparing expander free electrodes for lead acid battery and performance thereof
EP3404747A1
Carbon nanotube dispersion and use for same
EP3786110A1
Negative active material, lithium secondary battery including the material, and method of manufacturing the material
US10622631B2
Active carbon-based nanotube battery
US20050181282A1