Aluminum alloy heat treatment method based on selective laser melting forming

Through high-temperature direct aging heat treatment after selective laser melting and forming, the problem of improving the ductility of Al-Cu-Mg high-strength aluminum alloy formed by SLM has been solved, achieving significant elongation improvement and optimization of mechanical properties, and avoiding grain coarsening and mechanical properties. Performance degradation.

CN118808671APending Publication Date: 2024-10-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962642.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult to significantly improve the ductility of Al-Cu-Mg high-strength aluminum alloy formed by SLM in traditional heat treatment, and the secondary nano-precipitate phase introduced by alloying with Ti element may affect the mechanical properties.

Method used

A high-temperature direct aging heat treatment method based on laser selective melting and forming is adopted. The specific steps include computer drawing of a three-dimensional model, after laser selective melting and forming, aging heat treatment at 350°C for 2 hours, and air cooling to room temperature to optimize the grain morphology and precipitation phase. Improve the mechanical properties of alloys.

Benefits of technology

The ductility of Al-Cu-Mg aluminum alloy is significantly improved, with the elongation reaching 21.7±1.8%, maintaining high yield strength and tensile strength, while avoiding grain coarsening and deterioration of mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808671A_ABST
    Figure CN118808671A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal additive preparation, and particularly relates to a heat treatment method for an aluminum alloy based on selective laser melting forming. According to the heat treatment method, the crystal grain morphology and the evolution rule of each precipitated phase are obtained through high-temperature direct aging heat treatment, and the heat treatment method for the aluminum alloy based on selective laser melting forming with the excellent mechanical property is further obtained. The result of the embodiment shows that after the Al-Cu-Mg alloy prepared by the invention is subjected to high-temperature direct aging heat treatment at 350 DEG C for 2h / AC, the ductility of the Al-Cu-Mg alloy reaches 21.7 + / -1.8%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal additive manufacturing, and in particular relates to a heat treatment method for aluminum alloys formed by laser selective melting. Background Art

[0002] Laser Additive Manufacturing (LAM) has gradually become a rapid and precise forming technology for high-performance metal components due to its high manufacturing flexibility, high forming accuracy and good surface quality. Among them, Selective Laser Melting (SLM) can be used to form metal parts with extremely complex structures due to its small spot size and powder thickness, providing an important way for the integrated manufacturing of high-performance complex aluminum alloy components. During the SLM forming process, the cooling rate of the molten pool can reach 104-106℃ / s, and the rapid melting process in the molten pool can refine the intragranular substructure and enhance the matrix solid solution strengthening effect. In recent years, the preparation of complex and high-strength aluminum alloy parts by SLM technology has been valued in the fields of aerospace, transportation and other high-end equipment manufacturing.

[0003] However, the SLM forming of high-strength aluminum alloys still faces a series of challenges. The most critical problem is that traditional high-strength aluminum alloys are prone to thermal cracking during the forming process due to the wide solidification temperature range (such as the solidification temperature range of 2024Al alloy is about 134℃, and the solidification temperature range of 7050Al alloy is about 179℃), coupled with the high transient thermal stress inherent in SLM technology.

[0004] At present, the only aluminum alloys suitable for SLM forming are near-eutectic Al-Si alloys (AlSi 10 Mg、AlSi 12 ) and Al-Mg-Sc-Zr alloy. However, the mechanical properties of Al-Si alloy formed by SLM are usually lower than those of traditional medium and high strength aluminum alloys, and it is difficult to further strengthen it through heat treatment, and it cannot meet the application requirements of high-strength aluminum alloys. Airbus proposed a special Al-Mg-Sc-Zr alloy for LAM (Scalmalloy ) After heat treatment, the tensile properties are comparable to those of Al-Zn-Mg-Cu alloys, but the expensive price of the rare element Sc limits the promotion and application of this alloy.

[0005] Therefore, based on the previous work, we innovatively proposed a new type of Al-Cu-Mg-Si-Ti high-strength aluminum alloy for SLM. Different from the traditional cast Al-Cu-Mg alloy, the deposited Al-Cu-Mg-Si-Ti alloy presents a unique ultra-fine equiaxed crystal + columnar crystal heterogeneous structure. The average grain size of α-Al equiaxed crystal is 0.68±0.51μm, and more than 50% of the grain diameter does not exceed 1μm. The average grain size of α-Al columnar crystal is 1.69±0.98μm, and the maximum grain size exceeds 5μm. In addition, there are two nano-precipitated phases inside the matrix, one is the S'-Al2CuMg(Si) phase commonly found in Al-Cu-Mg alloys, with a length of about 52.09nm, a width of about 2nm, and a volume fraction of about 8.5vol.%, and the other is the short rod-shaped Q'-Al5Cu2Mg8Si7 phase, which has a length of about 6.06nm and a volume fraction of about 2.73vol.%. Its deposited room temperature tensile strength reaches 541±2MPa, and its yield strength reaches 473±8MPa, while maintaining an elongation of 10.9±1.2%.

[0006] The new Al-Cu-Mg-Si-Ti alloy belongs to the Al-Cu-Mg alloy system, which can be further strengthened by heat treatment to improve the mechanical properties of the alloy. However, the current SLM-formed Al-Cu-Mg alloy still mainly uses the T6 heat treatment system of "high temperature solution + low temperature aging" formulated for traditional deformed Al-Cu-Mg alloys, without considering the unique microstructure of the deposited sample caused by the rapid heating and cooling + reciprocating heat cycle of the SLM process, resulting in the performance potential of the SLM-formed Al-Cu-Mg alloy cannot be fully explored. For example, the ultrafine grains of the new Al-Cu-Mg-Si-Ti alloy formed by SLM will undergo dynamic recovery and recrystallization in the high temperature solution stage of the T6 heat treatment, resulting in significant coarsening of the grains and deterioration of the mechanical properties of the alloy; in addition, Ti element alloying may introduce secondary L12-Al3Ti nanoprecipitate phase, which can significantly improve the mechanical properties of the alloy.

[0007] (2) Research status of heat treatment system for Al-Cu-Mg high-strength aluminum alloys for SLM

[0008] In the study on heat treatment of SLM formed Zr alloyed modified Al-Cu-Mg alloy, Wang et al. studied the effect of direct aging (DA) heat treatment at 370℃, 7h / AC on the microstructural evolution and mechanical properties of SLM formed Al-Cu-Mg-Zr alloy. The study showed that DA heat treatment did not significantly change the microstructure of the sample at the grain scale, but promoted the precipitation of a large number of spherical nano-precipitated phases L12-Al3Zr in the crystal. Although the S' phase and GPB zone dissolved into the matrix during high-temperature direct aging, the yield strength of the DA state sample was further improved to 435MPa, and the elongation was only 7.5%.

[0009] For aluminum alloys modified by Ti, the precipitation of nano-precipitate phase L12-Al3Ti is also beneficial to improve the mechanical properties of the alloy. Hu et al. studied the effect of direct aging heat treatment on the microstructural evolution and mechanical properties of Ti-modified Al-5.0Cu alloy. The study found that heat treatment at 300°C would lead to the precipitation of nano-scale L12-Al3Ti precipitate phase, and the appearance of this precipitate phase increased the yield strength of the alloy by 19.9%. Judging from the research status of the above heat treatment system, there is currently no heat treatment method for aluminum alloys based on laser selective melting that can significantly improve the ductility of Al-Cu-Mg alloys. Summary of the invention

[0010] The purpose of the present invention is to provide a heat treatment method for aluminum alloy based on laser selective melting. The method provided by the present invention can significantly improve the ductility of Al-Cu-Mg aluminum alloy.

[0011] In order to achieve the above object, the present invention provides the following technical solutions:

[0012] The present invention provides a heat treatment method for aluminum alloy formed by laser selective melting, comprising the following steps:

[0013] The three-dimensional model required for forming is drawn by computer, and Al-Cu-Mg alloy is used as raw material to perform laser selective melting forming and heat treatment on the surface of the substrate;

[0014] The heat treatment comprises: performing aging heat treatment on the formed alloy and then air cooling it to room temperature; the temperature of the aging heat treatment is 350° C. and the holding time is 2 hours.

[0015] Preferably, the Al-Cu-Mg alloy comprises the following components by mass percentage: Cu 4.1-4.4%, Mg 2.9-3.2%, Si 1.9-2.2%, Ti 0.6-0.9% and the balance Al.

[0016] Preferably, the Al-Cu-Mg alloy comprises the following components by mass percentage: Cu 4.2%, Mg 3.04%, Si 2.01%, Ti 0.67% and the balance Al.

[0017] Preferably, the Al-Cu-Mg alloy is a spherical powder prepared by atomic gas atomization.

[0018] Preferably, the particle size of the spherical powder is 5 to 80 μm; the bulk density of the spherical powder is 1.35 to 1.45 g / cm 3 .

[0019] Preferably, the conditions for the laser selective melting forming include: laser power of 280 to 340 W, laser scanning rate of 100 to 1000 mm / s, and laser scanning spacing of 80 to 120 μm;

[0020] The thickness of each powder layer formed during the laser selective melting forming is 25-35 μm, and the inter-layer rotation angle of each powder layer formed during the laser selective melting forming is 65-70°.

[0021] Preferably, the substrate is an aluminum substrate; the substrate is preheated before use, and the preheating temperature is 120-180°C.

[0022] The present invention provides a heat treatment method for aluminum alloy formed by laser selective melting, comprising the following steps: using a computer to draw a three-dimensional model required for forming, using Al-Cu-Mg alloy as raw material, laser selective melting forming and heat treatment on the surface of a substrate; the heat treatment comprises: air cooling the formed alloy to room temperature after aging heat treatment; the temperature of the aging heat treatment is 350°C and the holding time is 2h. The present invention obtains the evolution law of the grain morphology and each precipitation phase through high-temperature direct aging heat treatment, and further obtains a heat treatment method for aluminum alloy formed by laser selective melting with excellent mechanical properties. The results of the embodiment show that the Al-Cu-Mg-Si-Ti alloy prepared by the present invention has an elongation of 21.7±1.8% after high-temperature direct aging heat treatment at 350°C and 2h / AC. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a hardness variation curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 during the direct aging heat treatment at 350°C;

[0024] Figure 2 This is an EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after high-temperature direct aging heat treatment at 350°C and 2h / AC;

[0025] Figure 3 This is a TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after being subjected to a high temperature direct aging heat treatment at 350°C and 2h / AC;

[0026] Figure 4 This is a room temperature tensile test result diagram of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after high temperature direct aging heat treatment at 350°C, 2h / AC;

[0027] Figure 5 This is a hardness change curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after being subjected to 500°C, 1h / WC solid solution treatment and aging at 190°C;

[0028] Figure 6 This is an EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC;

[0029] Figure 7 TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC;

[0030] Figure 8 This is a room temperature tensile test result diagram of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC;

[0031] Fig. 9 This is a hardness change curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 during the direct aging heat treatment at 190°C;

[0032] Fig.10 This is an EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low-temperature direct aging heat treatment at 190°C and 5h / AC;

[0033] Fig.11 This is a TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low-temperature direct aging heat treatment at 190°C, 5h / AC;

[0034] Fig.12This is a diagram showing the room temperature tensile test results of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low temperature direct aging heat treatment at 190°C, 5h / AC. DETAILED DESCRIPTION

[0035] The present invention provides a heat treatment method for aluminum alloy formed by laser selective melting, comprising the following steps:

[0036] The three-dimensional model required for forming is drawn by computer, and Al-Cu-Mg alloy is used as raw material to perform laser selective melting forming and heat treatment on the surface of the substrate;

[0037] The heat treatment comprises: performing aging heat treatment on the formed alloy and then air cooling it to room temperature; the temperature of the aging heat treatment is 350° C. and the holding time is 2 hours.

[0038] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0039] The invention adopts a computer to draw a three-dimensional model required for forming, uses Al-Cu-Mg alloy as raw material, and performs laser selective melting forming and heat treatment on the surface of a substrate.

[0040] In the present invention, the size of the three-dimensional model required for the forming is preferably 8×8×8 mm.

[0041] In the present invention, the Al-Cu-Mg alloy preferably includes the following components by mass percentage: Cu 4.1-4.4%, Mg 2.9-3.2%, Si 1.9-2.2%, Ti 0.6-0.9% and the balance Al, and further preferably includes the following components: Cu 4.2%, Mg 3.04%, Si 2.01%, Ti 0.67% and the balance Al.

[0042] In the present invention, the Al-Cu-Mg alloy is preferably a spherical powder prepared by atomic atomization. The present invention has no special limitation on the specific process of the atomic atomization method, and the method known to those skilled in the art can be adopted. In the present invention, the particle size of the spherical powder is preferably 5 to 80 μm, more preferably 15 to 53 μm, and more preferably 20 to 50 μm; the bulk density of the spherical powder is preferably 1.35 to 1.45 g / cm 3 , more preferably 1.38 to 1.42 g / cm 3 , more preferably 1.40 g / cm 3 .

[0043] In the present invention, the Al-Cu-Mg alloy is preferably dried before forming; the drying is preferably carried out in a vacuum drying oven; the drying temperature is preferably 120° C., and the drying time is preferably 4 hours.

[0044] In the present invention, the substrate is preferably an aluminum substrate; the substrate is also preferably preheated before use, and the preheating temperature is preferably 120-180°C.

[0045] In the present invention, the process of laser selective melting is preferably: placing the dried Al-Cu-Mg alloy into the powder baking cylinder of the SLM printer for laser selective melting. In the present invention, the conditions of laser selective melting preferably include: laser power of 280-340W, laser scanning rate of 100-1000mm / s, and laser scanning spacing of 80-120μm. In the present invention, the thickness of each layer of powder formed during the laser selective melting is preferably 25-35μm, and more preferably 30μm; the inter-layer rotation angle of each layer of powder formed during the laser selective melting is preferably 65-70°, and more preferably 67°.

[0046] In the present invention, the Al-Cu-Mg alloy sample is formed by laser selective melting, which can completely eliminate cracks and has no obvious pores or poor fusion defects. The sample density reaches 99.99%, and the tensile strength of the deposited sample at room temperature is 541±2MPa, the yield strength is 473±8MPa, and the elongation is 10.9±1.2%.

[0047] After the laser selective melting forming is completed, the present invention preferably further comprises cooling the formed Al-Cu-Mg alloy to room temperature and then taking it out; cleaning the taken out Al-Cu-Mg alloy, and separating the Al-Cu-Mg alloy formed by laser selective melting from the substrate by wire cutting. In the present invention, residual Al-Cu-Mg alloy powder can be removed by cleaning.

[0048] In the present invention, the heat treatment includes: performing aging heat treatment on the formed alloy and then air cooling to room temperature; the temperature of the aging heat treatment is 350°C and the holding time is 2h. In the present invention, the tensile strength of the heat-treated alloy at room temperature is 298±4.0MPa, the yield strength is 243.0±2.6MPa, and the elongation is 21.7±1.8%. The Al-Cu-Mg aluminum alloy with high plasticity can be prepared by the above high-temperature direct aging heat treatment system.

[0049] In order to further illustrate the present invention, a heat treatment method for aluminum alloy based on laser selective melting provided by the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0050] Example 1

[0051] The particle size of the prepared particles is 15-53 μm and the bulk density is 1.40 g / cm 3 Aluminum alloy powder, wherein the mass percentage of each element in the aluminum alloy powder is 4.5% Cu, 3.0% Mg, 2.0% Si, 0.7% Ti and the balance is aluminum.

[0052] The morphology of the aluminum alloy powder was observed under a scanning electron microscope, the phase composition of the aluminum alloy powder was determined by an X-ray diffractometer, and the composition and particle size of the powder were determined.

[0053] The three-dimensional model required for laser selective melting was drawn by computer, with a size of (8mm×8mm×8mm). The spherical powder was placed in a vacuum drying oven for drying, degassing and dehydration. The specific process was 120°C and kept warm for 4 hours.

[0054] The dried aluminum alloy powder was used as raw material, placed in the powder drying cylinder of the SLM printer, and the SLM printer was turned on for SLM forming. The printing parameters were: scanning spacing of 100 μm, layer thickness of 30 μm, scanning strategy of 67° rotation angle between adjacent layers, Al substrate preheating temperature of 150°C, laser power of 340 W, and scanning speed of 400 mm / s.

[0055] After completing the sample forming experiment, wait until the temperature of the forming chamber drops to room temperature, then take out the substrate and the sample, clean up the residual powder, and use wire cutting to separate the printed sample from the substrate.

[0056] The alloy formed by laser selective melting is subjected to aging heat treatment; the temperature of the aging heat treatment is 350° C., and after being kept at this temperature for 2 hours, it is naturally cooled to room temperature.

[0057] Comparative Example 1

[0058] Taking Example 1 as a benchmark, keeping the parameters before heat treatment unchanged, the formed alloy was subjected to solution heat treatment, water cooling, aging heat treatment and air cooling in sequence. The temperature of the solution heat treatment was 500°C, the holding time was 1h, the temperature of the aging heat treatment was 190°C, and after holding for 5h, it was naturally cooled to room temperature.

[0059] Comparative Example 2

[0060] Taking Example 1 as a benchmark, the parameters before heat treatment were kept unchanged, and the formed alloy was subjected to aging heat treatment at a temperature of 190° C. After keeping the temperature for 5 hours, the alloy was naturally cooled to room temperature.

[0061] Performance Testing

[0062] (1) The aluminum alloy samples prepared in Example 1 and Comparative Examples 1-2 were polished with 120, 200, 500, 1000, 1500, and 2000 grit sandpapers, and the phase compositions of the samples were determined.

[0063] (2) The aluminum alloys prepared in Example 1 and Comparative Examples 1 to 2 were polished with sandpaper of 120, 200, 500, 1000, 1500, and 2000 meshes, respectively, and polished with SiO2 polishing liquid. The deposited samples were characterized by SEM, EBSD, and TEM analysis (the samples used for EBSD testing were then subjected to ion polishing equipment to remove the surface stress layer).

[0064] (3) The aluminum alloys prepared in Example 1 and Comparative Examples 1 to 2 were machined according to the national standard tensile specimen size, and the block metal samples were processed into plate tensile specimens along the horizontal direction. The mechanical properties of the aluminum alloy plate tensile specimens prepared under different heat treatment conditions were tested at room temperature.

[0065] Figure 1 The hardness variation curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 during the direct aging process at 350°C. Figure 1 It can be concluded that after high-temperature direct artificial aging, the microhardness value of the sample is significantly lower than that of the deposited sample, and no obvious aging hardening process occurs. The hardness value reaches the highest value of 89.2±1.3HV after aging for 2 hours.

[0066] Figure 2 EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after high temperature direct aging heat treatment at 350°C, 2h / AC; Figure 2 It can be concluded that the microstructure consists of fine equiaxed α-Al crystals at the edge of the molten pool + columnar crystals inside the molten pool, indicating that the high-temperature direct artificial aging heat treatment at 350℃, 2h / AC will not cause large-scale recrystallization and obvious grain coarsening. The α-Al grain sizes in the fine and coarse grain areas are 0.8±0.6μm and 1.7±1.4μm, respectively, and the volume fraction of the columnar crystal area is 36.9vol.%.

[0067] Figure 3TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after high temperature direct aging heat treatment at 350°C, 2h / AC; Figure 3 It can be concluded that after high-temperature artificial aging treatment at 350℃, 2h / AC, the expected nano-L12-Al3Ti precipitate phase is not formed, and the high-density S' and Q' nano-precipitates precipitated in situ in the deposited sample dissolve back into the α-Al matrix.

[0068] Figure 4 The room temperature tensile test results of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Example 1 after high temperature direct aging heat treatment at 350°C, 2h / AC; Figure 4 It can be concluded that the yield strength, tensile strength and elongation of the samples treated with high temperature direct artificial aging are 243.0±2.6MPa, 298.2±4.0MPa and 21.7±1.8%, respectively. Although the strength has decreased significantly, the plasticity has increased significantly.

[0069] Figure 5 The hardness change curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after solution treatment at 500°C for 1h / WC and aging at 190°C is shown in FIG. Figure 5 It can be concluded that the solution heat-treated sample reaches the peak aging state when aged at 190℃ for 5 hours, and the peak aging hardness value is 135.4±3.5HV.

[0070] Figure 6 EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC; Figure 6 It can be concluded that the microstructure of the T6 heat-treated alloy is composed of coarse α-Al equiaxed crystals and fine α-Al equiaxed crystals. The average grain size reaches 15.1±24.4μm, and its statistical standard deviation also increases significantly, which indicates that the grain size varies greatly. The number fraction of equiaxed crystals with a grain size of less than 5μm reaches 60.7%, but its volume fraction accounts for only 15.7%, and the largest grain size can reach 150μm.

[0071] Figure 7 TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC; Figure 7It can be concluded that after T6 heat treatment, there are two high-density nano-precipitate phases in the matrix, one is a long needle-like θ' precipitate phase with a length of 30-100nm, which is enriched in Cu element, and the other is a short rod-like Q' nano-precipitate phase.

[0072] Figure 8 The room temperature tensile test results of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 1 after T6 heat treatment at 500°C, 1h / WC+190°C, 5h / AC; Figure 8 It can be concluded that after heat treatment, the yield strength, tensile strength and elongation of the sample are 390.6±9.8MPa, 474.0±8.7MPa and 11.8±0.1%, respectively.

[0073] Fig. 9 The hardness variation curve of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 during the direct aging process at 190°C. Fig. 9 It can be concluded that the microhardness value of the sample increases continuously with the extension of aging time until the aging time is 5h, reaching the peak aging state. At this time, the microhardness value of the sample is 177.4±1.3HV.

[0074] Fig.10 This is the EBSD scanning image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low-temperature direct aging heat treatment at 190°C, 5h / AC; Fig.10 It can be concluded that the microstructure of the low temperature direct artificial aging sample is a dual-state grain structure of α-Al equiaxed crystals + columnar crystals. The grain sizes of α-Al equiaxed crystals and columnar crystals are 0.7±0.5μm and 1.7±1.2μm, respectively.

[0075] Fig.11 TEM image of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low-temperature direct aging heat treatment at 190°C, 5h / AC; Fig.11 It can be concluded that after low-temperature direct artificial aging heat treatment, there are still two nano-precipitated phases with different morphologies in the α-Al matrix of the sample, namely the long needle-like S' phase and the short rod-like Q' phase, and the density of the short rod-like Q' phase increases significantly.

[0076] Fig.12 The room temperature tensile test results of the deposited Al-Cu-Mg-Si-Ti alloy prepared in Comparative Example 2 after low temperature direct aging heat treatment at 190°C, 5h / AC; Fig.12It can be concluded that the yield strength, tensile strength and elongation of the low-temperature direct artificial aging specimens are 517.1±6.3MPa, 552.2±1.5MPa and 5.9±0.7%, respectively.

[0077] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A heat treatment method for aluminum alloy formed by laser selective melting, characterized in that: The following steps are involved: The three-dimensional model required for forming is drawn by computer, and Al-Cu-Mg alloy is used as raw material to perform laser selective melting forming and heat treatment on the surface of the substrate; The heat treatment comprises: performing aging heat treatment on the formed alloy and then air cooling it to room temperature; the temperature of the aging heat treatment is 350° C. and the holding time is 2 hours.

2. The heat treatment method according to claim 1, characterized in that The Al-Cu-Mg alloy comprises the following components by mass percentage: 4.1-4.4% Cu, 2.9-3.2% Mg, 1.9-2.2% Si, 0.6-0.9% Ti and the balance Al.

3. The heat treatment method according to claim 2, characterized in that: The Al-Cu-Mg alloy comprises the following components by mass percentage: 4.2% Cu, 3.04% Mg, 2.01% Si, 0.67% Ti and the balance Al.

4. The heat treatment method according to claim 1, characterized in that: The Al-Cu-Mg alloy is a spherical powder prepared by atomic gas atomization.

5. The heat treatment method according to claim 4, characterized in that: The particle size of the spherical powder is 5 to 80 μm; the bulk density of the spherical powder is 1.35 to 1.45 g / cm 3 .

6. The heat treatment method according to claim 1, characterized in that: The conditions of the laser selective melting forming include: laser power of 280-340W, laser scanning rate of 100-1000mm / s, and laser scanning spacing of 80-120μm; The thickness of each powder layer formed during the laser selective melting forming is 25-35 μm, and the inter-layer rotation angle of each powder layer formed during the laser selective melting forming is 65-70°.

7. The heat treatment method according to claim 1, characterized in that: The substrate is an aluminum substrate; the substrate is preheated before use, and the preheating temperature is 120-180°C.