A method for machining TB9 titanium alloy cylindrical helical compression springs
By adopting TB9 titanium alloy material and controlling the aging treatment parameters, the problems of length attenuation and stress relaxation in cylindrical helical compression springs were solved, realizing corrosion-resistant and lightweight TB9 titanium alloy springs, and improving service life and parameter consistency.
Patent Information
- Application Number
- CN202411029132.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing cylindrical helical compression springs exhibit length attenuation and stress relaxation during use, are prone to corrosion, and fail to meet the lightweight requirements of the aerospace industry.
Cylindrical helical compression springs are machined using TB9 titanium alloy material. By controlling parameters such as the temperature and time of aging treatment and the furnace exit temperature, the tensile strength is ensured to be between 1300MPa and 1350MPa. Combined with shot peening and dynamic fatigue testing, the processing parameters are adjusted to meet the service life requirements.
A TB9 titanium alloy spring with low stress relaxation resistance and low length decay was achieved, meeting the requirements of corrosion resistance and lightweight, and improving the service life and parameter consistency of the spring.
Smart Images

Figure CN118809094B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of spring processing technology, specifically relating to a method for processing a TB9 titanium alloy cylindrical helical compression spring. Background Technology
[0002] As a mechanical component, springs are frequently subjected to complex loads and undergo reciprocating deformation and reset movements during use to provide cushioning and shock absorption. In particular, buffer springs and firing springs are used in complex environments, operate at high frequencies, and have long service lives, requiring them to have high fatigue life and a certain degree of corrosion resistance. If used in the aerospace field, lightweight design is also a necessary consideration.
[0003] Cylindrical helical compression springs are the most common type of spring. Currently, they are mainly made of carbon spring steel wire, alloy spring steel wire, and stainless steel spring steel wire. However, springs made of these materials suffer from length attenuation and stress relaxation during use, which affects the life of the spring. They are also prone to corrosion and cannot meet the lightweight requirements of the aerospace field. Summary of the Invention
[0004] To address the problems of existing cylindrical helical compression springs, such as length attenuation and stress relaxation, susceptibility to corrosion, and inability to meet lightweight requirements, this invention proposes a processing method for TB9 titanium alloy cylindrical helical compression springs. The aim is to provide a spring with low stress relaxation resistance, low length attenuation, and simultaneously meet the requirements of corrosion resistance and lightweight design.
[0005] The inventive concept of this invention:
[0006] First, this invention proposes using TB9 titanium alloy to process cylindrical helical compression springs, which can achieve the expected weight reduction effect. Compared with springs of the same specifications, the weight can be reduced by 42.55%. Moreover, TB9 titanium alloy material has strong corrosion resistance. Compared with carbon spring steel wire and alloy spring steel wire, titanium alloy springs do not require surface anti-corrosion treatment and can meet general use requirements by relying on the material's own anti-corrosion properties.
[0007] Furthermore, during the testing process, the applicant discovered that cylindrical helical compression springs made of TB9 titanium alloy were prone to failing to meet test parameters and batch defects during fatigue testing. Through extensive analysis, the applicant found that this was because the tensile strength of the springs after aging treatment was too high, too close to the limit value of 1400 MPa, resulting in poor spring life. To address this issue, the applicant considered controlling parameters such as the aging treatment temperature, time, and furnace exit temperature during the heat treatment process to ensure that the tensile strength of the obtained springs does not approach the limit value, thereby guaranteeing that the parameters of the finally processed springs meet the requirements and improving spring life.
[0008] To achieve the above objectives, the technical solution provided by this invention is:
[0009] A method for machining a TB9 titanium alloy cylindrical helical compression spring includes the following steps:
[0010] Step 1, Material preparation: Prepare materials using solution-treated TB9 titanium alloy wire.
[0011] Step 2, Winding the spring: Wind the wire into a cylindrical helical compression spring body;
[0012] Step 3, Grinding the end faces: Grind both end faces of each spring;
[0013] Step 4, Aging treatment: Place the spring in a vacuum heat treatment furnace and age it for a predetermined time at a preset temperature. After cooling in the furnace, remove the spring so that its tensile strength is between 1300MPa and 1350MPa.
[0014] Step 5, high-pressure treatment: Thread the spring onto the mandrel and compress the spring to put it in a compressed state, and hold it for a predetermined time;
[0015] Step 6, shot peening: Use steel shot smaller than 1 / 2 the diameter of the wire to perform shot peening on the spring, requiring a shot peening coverage of more than 90%;
[0016] Step 7, Dynamic Fatigue Test: Randomly select 3% of the springs, apply a periodic load to the springs, and stop the machine after a predetermined number of cycles to check the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts and retest. If any part still does not meet the requirement after the second test, the batch of products is deemed unqualified. Then, adjust the aging treatment temperature, time and furnace exit temperature in Step 4 for the next batch of parts until the parts meet the requirements.
[0017] Furthermore, in step 2, an automatic spring winding machine is used to wind the spring body.
[0018] Furthermore, in step 2, the spring body is wound using a lathe with a core winding method.
[0019] Furthermore, in step 3, a spring grinding machine is used to grind the end face of the spring.
[0020] Furthermore, in step 3, the spring end face is manually ground using a grinding wheel.
[0021] Furthermore, in step 3, if the grinding amount is too large, the two end faces of the spring body are first cut by wire cutting, and then fine grinding is performed.
[0022] The advantages of this invention are:
[0023] 1. The TB9 titanium alloy cylindrical helical compression spring processing method of the present invention uses solution-treated TB9 titanium alloy wire to manufacture the cylindrical helical compression spring. After the spring body is wound and formed, the spring end face is ground and then heat-treated. During the aging treatment, the tensile strength is controlled to not approach the limit value, between 1300MPa and 1350MPa. Finally, the life of the spring is checked by dynamic fatigue test. If it is not qualified, the temperature and time of aging treatment are adjusted to make the part meet the life requirements. Thus, a cylindrical helical compression spring can be obtained with a simple process. During the service life, the free length and stiffness of the spring hardly decrease or relax, achieving the purpose of anti-stress relaxation and anti-attenuation. At the same time, the TB9 titanium alloy material can meet the requirements of corrosion resistance and lightweight.
[0024] 2. The spring winding and end face grinding processes in this invention can be adapted to both large-batch and small-batch production modes, making the process highly adaptable. Attached Figure Description
[0025] The above and / or other features and advantages of the present invention will become more readily understood from the following description with reference to the accompanying drawings, which are not drawn to scale and some features are enlarged or reduced to show details of specific parts.
[0026] Figure 1 This is a flowchart of the TB9 titanium alloy cylindrical helical compression spring processing method of the present invention;
[0027] Figure 2 This is a simplified diagram of the parts obtained in an example of the present invention;
[0028] Figure 3 These are images of parts that fractured after fatigue testing, obtained in an example of this invention.
[0029] Figure 4 These are images of the fracture surface of a part obtained in an example of the present invention. Detailed Implementation
[0030] The present invention will now be described in detail with reference to the accompanying drawings and exemplary embodiments thereof. It should be noted that the following detailed description of the present invention is for illustrative purposes only and is not intended to limit the scope of the invention.
[0031] This invention provides a method for processing a cylindrical helical compression spring made of TB9 titanium alloy. This method uses TB9 titanium alloy to process a cylindrical helical compression spring, which can obtain a spring with low stress relaxation resistance, low length attenuation, and simultaneously meet the requirements of corrosion resistance and lightweight.
[0032] Reference Figure 1The TB9 titanium alloy cylindrical helical compression spring processing method, as an exemplary embodiment of the present invention, may include the following steps:
[0033] Step S1, Material preparation: Prepare materials using solution-treated TB9 titanium alloy wire.
[0034] Step S2, Winding the spring: Winding the wire into a cylindrical helical compression spring body;
[0035] Step S3, Grinding end faces: Grind both end faces of each spring;
[0036] Step S4, Aging treatment: Place the spring in a vacuum heat treatment furnace and age it for a predetermined time at a preset temperature. After cooling in the furnace, remove the spring so that its tensile strength is between 1300MPa and 1350MPa.
[0037] Step S5, strong pressure treatment: Thread the spring onto the mandrel, compress the spring to put it in a compressed state, and hold it for a predetermined time;
[0038] Step S6, shot peening: Use steel shot smaller than 1 / 2 the diameter of the wire to perform shot peening on the spring, requiring a shot peening coverage of more than 90%;
[0039] Step S7, Dynamic Fatigue Test: Randomly select 3% of the springs, apply a periodic load to the springs, stop the machine after a predetermined number of cycles, and check the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts and retest. If there are still parts that do not meet the requirements after the second test, the batch of products is determined to be unqualified. Then, for the next batch of parts, adjust the aging treatment temperature, time and furnace exit temperature in step S4 until the parts meet the requirements.
[0040] In step S1, TB9 titanium alloy wire is used. This material has the advantages of good corrosion resistance, high fatigue life, and low density, with a density of 4.51 g / cm3, which is 57.45% of the density of commonly used steel. The wire is in a solution-treated state, which has good processability and can eliminate the need for a solution treatment process after spring forming, thus avoiding deformation during the solution treatment of the spring.
[0041] In the spring winding process of step S2, automatic spring winding machines are preferred because they have the advantages of high production efficiency, good product consistency, and are suitable for mass production. When the production batch is small, in order to save materials, the core winding method on a lathe can be used.
[0042] In step S3, a spring grinding machine is preferred for grinding the end face. Its advantages are good parallelism and perpendicularity of the two end faces, high production efficiency, good product consistency, and suitability for mass production. When the production batch is small or there is no automatic spring winding machine, a grinding wheel can be used instead of a spring grinding machine for manual grinding in order to save costs.
[0043] In addition, when the grinding amount is too large, wire EDM can be used for rough cutting first, and then fine grinding can be performed to achieve the required dimensions. The heat-affected surface of the wire EDM must be ground off to eliminate the potential for micro-cracks in the wire EDM.
[0044] The aging treatment in step S4 must be performed after grinding the end face. This eliminates the stress generated by grinding and controls the strength of the spring material within a certain range, maximizing the spring's lifespan. A vacuum heat treatment furnace is used, and the spring is aged at a specific temperature for a certain time. After exiting the furnace, the tensile strength of the material is between 1300 MPa and 1350 MPa. The spring surface has a good gloss, with no obvious oxidation or discoloration, and does not approach the ultimate tensile strength of 1400 MPa, ensuring that the parts meet the testing requirements in the final fatigue test.
[0045] In step S5, the high-pressure treatment is to reduce stress concentration, which can effectively improve the life of the spring.
[0046] Before shot peening in step S6, the spring must not be subjected to force or deformation; otherwise, irreversible deformation will occur after shot peening. Shot peening can eliminate defects such as microcracks on the material surface and reduce stress concentration. Furthermore, it can create a new stress layer on the material surface, achieving the purpose of applying prestress. This prestress can effectively counteract the load on the spring during use. Shot peening can significantly improve the service life of the spring.
[0047] Step S7 verifies whether the lifespan of the processed parts meets the requirements. This involves applying a periodic load under certain conditions to the spring and then testing its length and load. This verifies length attenuation and stress relaxation. The test parameters are then checked to ensure they are not less than specified values. For a batch, if one part in 3% of the springs breaks or fails to meet requirements during the test, the sample size is doubled and the test is repeated. If any part still fails to meet requirements, the entire batch is considered unqualified. In this case, for the next batch of parts, the aging treatment temperature and time need to be adjusted to ensure the spring lifespan meets the requirements.
[0048] As described above, this invention provides a simple process for obtaining cylindrical helical compression springs. During the spring's service life, its free length and stiffness show almost no decrease or relaxation, achieving resistance to stress relaxation and attenuation. Furthermore, the TB9 titanium alloy material meets the requirements for corrosion resistance and lightweight design. In addition, the spring winding and end-face grinding processes in this invention can be adapted to both large-batch and small-batch production models, demonstrating strong process applicability.
[0049] The following examples will further illustrate the processing method of the TB9 titanium alloy cylindrical helical compression spring provided by this invention.
[0050] In this example, such as Figure 2As shown, the dimensions of the spring part to be machined are: spring mean diameter D = 9.23 mm, titanium alloy wire diameter d = Φ2.27 mm, spring pitch t = 4.69 mm, spring free length H0 = 55 ± 1 mm, spring preload length H1 = 46 mm, spring working length H2 = 34 mm, and spring compression height H. b =30.8mm, spring load F1=140±10N, spring load F2=328±20N, load F when spring is compressed b =376.4N, total number of spring coils n1 = 13 ± 0.75 coils, effective coils n = 11 coils.
[0051] The processing procedure is as follows:
[0052] Process 1, Material preparation: TB9 solution-treated titanium wire with a diameter of Φ2.27mm is used. The whole coil of material is prepared. The material passes the incoming inspection and the actual wire diameter is Φ2.29mm, which meets the tolerance requirements.
[0053] Process 2, Spring Winding: The spring is wound using a 1A62 lathe with a mandrel diameter of Φ6.4, and the pitch is designed to account for deformation after compression. After cutting a single spring on the lower lathe, the total number of turns n1 = 13 to 13.15 turns.
[0054] Step 3, Grinding the end face: Grind the end face manually with a grinding wheel. The support rings on both ends are 3 / 4 turns. After grinding the end face, the spring H0 is reserved for the deformation after compression.
[0055] Step 4, Aging Treatment: The sample is aged in a vacuum heat treatment furnace at 500℃ for 5 hours. It is then cooled to 100℃ in the furnace before being removed from the furnace. The tensile strength σ of the sample is then tested. b =1320 MPa, yield strength σ s =1215 MPa.
[0056] Step 5, high-pressure treatment: Thread the spring onto the Φ6.4 mandrel and press it to Hb and hold for 24 hours.
[0057] Step 6, shot peening: use 1mm steel shot and 39A current for 10 minutes of rolling shot peening, with a shot peening coverage of over 95%.
[0058] Step 7, Parts Inspection: Randomly select 2 finished parts for inspection. The product dimensions must conform to the drawing requirements, as detailed below:
[0059] Part Number Length H0 Diameter D1 Load P2 ① 54.5 11.51 330 ② 54.7 11.51 332
[0060] Step 8, Fatigue Test: A fatigue test is conducted on the two parts mentioned above. Test conditions: frequency 710 cycles / minute, amplitude H1~H2, room temperature, mandrel Φ6.3. The test is performed after 100,000 cycles, followed by a shutdown. The spring length decay (i.e., the change in the spring's unfolded length H0) and stress relaxation (i.e., the spring load P2) are monitored until the spring fractures due to fatigue. The spring fracture failure and fracture surface conditions are as follows: Figure 3 and Figure 4 As shown. The detection data is as follows:
[0061]
[0062] The results in the table above show that the parts produced by the TB9 titanium alloy cylindrical helical compression spring processing method of the present invention meet the drawing requirements, and the process is feasible. Fatigue tests prove that the length and stiffness of the TB9 titanium alloy spring reach a stable state within 30 minutes under the test environment, and after stabilization, the length and stiffness remain unchanged within 60 minutes, that is, the anti-stress relaxation and length attenuation effects are obvious.
[0063] Finally, it should be noted that the features mentioned and / or shown in the above description of exemplary embodiments of the present invention can be combined in the same or similar manner with one or more other embodiments, combined with features in other embodiments, or substituted for corresponding features in other embodiments. These combined or substituted technical solutions should also be considered to be included within the scope of protection of the present invention.
Claims
1. A method for machining a TB9 titanium alloy cylindrical helical compression spring, characterized in that, Includes the following steps: Step 1, Material preparation: Prepare materials using solution-treated TB9 titanium alloy wire. Step 2, Winding the spring: Wind the wire into a cylindrical helical compression spring body; Step 3, Grinding the end faces: Grind both end faces of each spring; Step 4, Aging treatment: Place the spring in a vacuum heat treatment furnace and age it at 500℃ for 5 hours. After cooling to 100℃ in the furnace, remove the spring to ensure that the tensile strength of the spring is between 1300MPa and 1350MPa, so as to avoid the tensile strength being too close to the limit value of 1400MPa. Step 5, high-pressure treatment: Thread the spring onto the mandrel and compress the spring to put it in a compressed state, and hold it for a predetermined time; Step 6, shot peening: Use steel shot smaller than 1 / 2 the diameter of the wire to perform shot peening on the spring, requiring a shot peening coverage of more than 90%; Step 7, Dynamic Fatigue Test: Randomly select 3% of the springs, apply a periodic load to the springs, and stop the machine after a predetermined number of cycles to check the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts and retest. If any part still does not meet the requirement after the second test, the batch of products is deemed unqualified. For the next batch of parts, adjust the aging treatment temperature, time and furnace exit temperature in Step 4 until the parts meet the requirements.
2. The method for processing TB9 titanium alloy cylindrical helical compression springs according to claim 1, characterized in that: In step 2, an automatic spring winding machine is used to wind the spring body.
3. The method for processing TB9 titanium alloy cylindrical helical compression springs according to claim 1, characterized in that: In step 2, the spring body is wound using a lathe with a core winding method.
4. The method for processing TB9 titanium alloy cylindrical helical compression springs according to claim 1 or 2, characterized in that, In step 3, a spring grinding machine is used to grind the end face of the spring.
5. The method for processing TB9 titanium alloy cylindrical helical compression springs according to claim 1 or 2, characterized in that: In step 3, the end face of the spring is manually ground using a grinding wheel.
6. The method for processing TB9 titanium alloy cylindrical helical compression springs according to claim 1 or 2, characterized in that: In step 3, if the grinding amount is too large, the two end faces of the spring body are first cut by wire cutting, and then fine grinding is performed.
Citation Information
Patent Citations
High temperature spring processing technology
CN104607880A