Jasmine flower shaving board and preparation method thereof
By using jasmine mixture and modified adhesive in particleboard, combined with the use of composite moisture-proof agent, the problem of expansion and insufficient mechanical properties of jasmine particleboard in an environment with changing humidity is solved, achieving high durability and excellent mechanical properties of the particleboard. .
Patent Information
- Application Number
- CN202411150186.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-22
AI Technical Summary
Jasmine particleboard is prone to expansion or contraction in an environment with changing humidity, which affects the dimensional stability and mechanical properties. The strength of jasmine fiber is weak, which affects the performance of the particleboard.
Jasmine particleboard is made of wood shavings, jasmine mixture, modified phenolic resin or modified urea-formaldehyde resin adhesive and composite moisture-proof agent. The dosage of jasmine mixture is 14%-16%, the dosage of glue is 8%-12%, and the composite moisture-proof agent The dosage is 3%-6%, in which the composite moisture-proof agent consists of silane moisture-proof agent, paraffin emulsion and nano-silica, which is solidified by hot-pressing treatment.
It significantly reduces the hygroscopicity of jasmine particleboard and improves its durability and mechanical properties, making it widely used and of high economic value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of artificial boards, and in particular relates to a jasmine particle board and a preparation method thereof. Background Art
[0002] Artificial boards are made of wood or other non-wood plants as raw materials. After being separated into various unit materials through certain mechanical processing, adhesives and other additives are applied to glue them together to form boards or molded products. They mainly include three categories of products: plywood, particleboard and fiberboard, and there are hundreds of extended products and deep-processed products. Among them, particleboard is also called particle board, bagasse board, and solid wood particle board. Particleboard is a board made of wood shavings or wood fiber materials with glue applied. Particleboard can be processed using small firewood, branches and wood processing residues from fast-growing forests as raw materials. It can replace plywood, make full use of forestry resources, and reduce the felling of forest resources. It is an important development direction of the artificial board industry.
[0003] In recent years, as consumers' requirements for artificial boards continue to increase, the smell of particleboard has become a factor in consumer choice. In the production process of particleboard, the wood species used for particleboard is the main source of the smell of particleboard. However, at the same time, due to the restrictions of the wood species, the selectivity of the smell of particleboard is insufficient. Therefore, in order to increase the selectivity of the smell of particleboard, some different plants will be added in the production process of particleboard. Through the smell of different plants, the particleboard can get a smell other than wood, which can provide consumers with new choices.
[0004] Jasmine has a fragrant and refreshing smell and is deeply loved by people. Adding jasmine organs, such as roots and stems, to particleboard can make the particleboard have the fragrance of jasmine, thereby enhancing the added value of the product and user experience. However, since jasmine plant fiber has strong hygroscopicity, when it is added to particleboard, it will cause the particleboard to expand or contract in an environment with changing humidity, thereby causing dimensional changes and deformation, affecting the performance of the particleboard.
[0005] In addition, due to the different densities of the jasmine mixture and the particleboard wood, the overall density of the particleboard will change, and the fiber structure of the plant fiber of the jasmine mixture has weak strength and rigidity, which will affect the mechanical properties of the particleboard. Summary of the invention
[0006] The object of the present invention is to provide a jasmine particleboard and a preparation method thereof, so as to solve the technical problems raised in the above background technology.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A jasmine particleboard is made of the following raw materials: wood shavings, a jasmine mixture, an adhesive, and a composite moisture-proof agent. The amount of the jasmine mixture is 14%-16% of the mass of the wood shavings; the amount of the adhesive is 8%-12% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 3%-6% of the mass of the wood shavings.
[0009] Furthermore, the jasmine mixture is a mixture obtained by crushing and mixing the stems, stalks, leaves and flowers of jasmine.
[0010] Furthermore, the adhesive is one of modified phenolic resin or modified urea-formaldehyde resin; the modified phenolic resin and modified urea-formaldehyde resin are modified by melamine, have the advantages of low odor, low formaldehyde and high strength, can reduce the influence of the odor of the adhesive itself on the odor of the particleboard, and make the particleboard retain the odor of itself and the jasmine mixture.
[0011] Furthermore, the composite moisture-proofing agent is prepared from silane moisture-proofing agent: paraffin emulsion: inorganic mineral matter in a mass ratio of 4-5:3-4:1-2.
[0012] Furthermore, the silane moisture-proofing agent is one of methyltriethoxysilane, alkyltrichlorosilane and vinyltriethoxysilane.
[0013] Furthermore, the paraffin in the paraffin emulsion is fully refined paraffin, and the concentration of the paraffin emulsion is 10-20%; paraffin is divided into fully refined paraffin, semi-refined paraffin and crude paraffin, semi-refined paraffin and crude paraffin contain impurities and odors, and will release pungent odors, thereby affecting the odor of the particle board, while fully refined paraffin has no mechanical impurities and moisture, no odor, and will not affect the odor of the particle board.
[0014] Furthermore, the inorganic mineral is one of nano silicon dioxide and nano aluminum oxide.
[0015] Furthermore, the preparation method of the composite moisture-proofing agent comprises the following steps:
[0016] S1: dissolving the silane moisture-proofing agent in a solvent, stirring and mixing, and obtaining a silane moisture-proofing agent solution;
[0017] S2: dissolving the inorganic mineral in a solvent, adding a polyethylene glycol dispersant, and then performing ultrasonic dispersion to obtain an inorganic mineral solution;
[0018] S3: mixing and stirring the silane moisture-proofing agent solution obtained in S1 and the inorganic mineral solution obtained in S2, slowly adding the paraffin emulsion during the stirring process, and mixing them evenly to obtain a mixed solution;
[0019] S4: Stabilizing the mixed solution obtained in S3 to obtain a composite moisture-proofing agent.
[0020] Furthermore, the stabilization treatment method is: firstly heat the mixed solution at 60-80°C for 1-2h, and then cool the heated mixed solution at 20-30°C; through the stabilization treatment, each component is fully reacted to form a stable chemical bond, and then the structure of the composite moisture-proof agent is stabilized by cooling, thereby improving the uniformity, stability and durability of the composite moisture-proof agent.
[0021] A method for preparing a jasmine particleboard comprises the following steps:
[0022] S1: drying the wood shavings and the jasmine mixture to a certain moisture content respectively; wherein the jasmine mixture is vacuum freeze-dried to maximize the retention of the main aroma substances of the jasmine;
[0023] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0024] S3: Evenly spread the glue-mixed wood shavings in a mold, perform heat-pressing treatment, solidify the adhesive, and obtain a jasmine particleboard.
[0025] Furthermore, in step S1, the mixture of wood shavings and jasmine flowers is dried to a moisture content of 5-8%.
[0026] Furthermore, in step S3, the temperature of the hot pressing treatment is 180-220° C., the pressure is 3-5 MPa, and the treatment time is 5-10 min.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. By adding a jasmine mixture, the present invention can make the prepared particleboard have the fragrance of jasmine, and at the same time can improve the influence of the hygroscopicity of jasmine fiber on the particleboard, improve the durability of the particleboard, and has excellent mechanical properties, wide application scenarios and high economic value.
[0029] 2. In the composite moisture-proofing agent of the present invention, silane moisture-proofing agent, paraffin emulsion and nano-silicon dioxide are used together. The silane moisture-proofing agent reacts with the hydroxyl groups in cellulose and hemicellulose to form silicon-oxygen bonds, forming a stable hydrophobic layer on the fiber surface to prevent water molecules from combining with cellulose and hemicellulose, thereby reducing hygroscopicity. The paraffin emulsion reduces the adsorption and retention of water by forming a hydrophobic film on the fiber surface. The paraffin molecules can cover the cell fibers and porous structures to prevent water from entering the interior of the fibers. Nano-alumina has an extremely high surface area and adsorption capacity, and can be combined with silane moisture-proofing agent and paraffin emulsion to enhance their adhesion and stability on the fiber surface. The addition of nano-alumina can improve the dispersibility and uniformity of the moisture-proofing agent, thereby enhancing the overall moisture-proofing effect. Therefore, silane desiccant and paraffin emulsion can form a double hydrophobic protective layer on the fiber surface to enhance the moisture-proof effect. Silane desiccant improves the hydrophobicity of the fiber through chemical bonding, paraffin emulsion prevents moisture penetration by forming a physical barrier, and nano-alumina improves the adhesion and stability of the desiccant. The three are used together to synergistically enhance their effectiveness and significantly reduce hygroscopicity.
[0030] 1. The nano silicon dioxide in the composite moisture-proofing agent of the present invention can not only improve the moisture-proof performance of the composite moisture-proofing agent, but also fill the pores inside and between the fibers, reduce the defects in the material, thereby improving the strength and rigidity of the fibers. At the same time, the nano silicon dioxide particles can form a uniform coating on the fiber surface, increase the interface bonding force between the fiber and the matrix, thereby improving the strength and rigidity of the fibers, thereby reducing the influence of the weak strength of the jasmine fiber on the mechanical properties of the particleboard, and improving the mechanical properties of the jasmine particleboard. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clear, preferred embodiments are given to further describe the present invention in detail. However, it should be noted that many details listed in the specification are only for the purpose of enabling readers to have a thorough understanding of one or more aspects of the present invention, and these aspects of the present invention can be implemented even without these specific details.
[0032] A jasmine particleboard is made of the following raw materials: wood shavings, a jasmine mixture, an adhesive, and a composite moisture-proof agent. The amount of the jasmine mixture is 14%-16% of the mass of the wood shavings; the amount of the adhesive is 8%-12% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 3%-6% of the mass of the wood shavings.
[0033] The jasmine flower mixture is a mixture obtained by crushing and mixing stems, stalks, leaves and flowers of jasmine flowers.
[0034] The adhesive is one of modified phenolic resin and modified urea-formaldehyde resin.
[0035] The composite moisture-proofing agent is prepared from silane moisture-proofing agent: paraffin emulsion: inorganic mineral matter in a mass ratio of 4-5:3-4:1-2.
[0036] The silane moisture-proofing agent is one of methyltriethoxysilane, alkyltrichlorosilane and vinyltriethoxysilane.
[0037] The paraffin in the paraffin emulsion is fully refined paraffin, and the concentration of the paraffin emulsion is 10-20%.
[0038] The inorganic mineral is one of nano silicon dioxide and nano aluminum oxide.
[0039] A method for preparing a jasmine particleboard comprises the following steps:
[0040] S1: Drying the wood shavings and the jasmine mixture separately to a moisture content of 5-8%;
[0041] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0042] S3: Evenly spread the glue-mixed wood shavings in a mold, and perform hot pressing treatment for 5-10 minutes at a temperature of 180-220° C. and a pressure of 3-5 MPa to solidify the adhesive to obtain a jasmine particleboard.
[0043] The following is described by more specific embodiments:
[0044] Example 1
[0045] A jasmine particleboard is made from the following raw materials: wood shavings, a jasmine mixture, a modified phenolic resin adhesive, and a composite moisture-proof agent; the amount of the jasmine mixture is 14% of the mass of the wood shavings; the amount of the adhesive is 10% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 6% of the mass of the wood shavings.
[0046] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:2.
[0047] A method for preparing a jasmine particleboard comprises the following steps:
[0048] S1: drying the wood shavings and the jasmine mixture separately to a moisture content of 6%;
[0049] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0050] S3: Evenly spread the glue-mixed wood shavings in a mold, and perform hot pressing for 10 minutes at a temperature of 200° C. and a pressure of 5 MPa to solidify the adhesive, thereby obtaining a jasmine particleboard.
[0051] Example 2
[0052] A jasmine particleboard is made of the following raw materials: wood shavings, a jasmine mixture, a modified phenolic resin adhesive, and a composite moisture-proof agent; the amount of the jasmine mixture is 15% of the mass of the wood shavings; the amount of the adhesive is 8% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 4% of the mass of the wood shavings.
[0053] The composite moisture-proofing agent is prepared from methyltriethoxysilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 18%: nano-alumina in a mass ratio of 4:3:2.
[0054] A method for preparing a jasmine particleboard comprises the following steps:
[0055] S1: drying the wood shavings and the jasmine mixture separately to a moisture content of 5%;
[0056] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0057] S3: Evenly spread the glue-mixed wood shavings in a mold, and perform hot pressing treatment for 8 minutes at a temperature of 190° C. and a pressure of 4 MPa to solidify the adhesive to obtain a jasmine particleboard.
[0058] Example 3
[0059] A jasmine particleboard is made from the following raw materials: wood shavings, a jasmine mixture, a modified urea-formaldehyde resin adhesive, and a composite moisture-proofing agent; the amount of the jasmine mixture is 16% of the mass of the wood shavings; the amount of the adhesive is 12% of the mass of the wood shavings; and the amount of the composite moisture-proofing agent is 3% of the mass of the wood shavings.
[0060] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 12%: nano-alumina in a mass ratio of 4:4:1.
[0061] A method for preparing a jasmine particleboard comprises the following steps:
[0062] S1: drying the wood shavings and the jasmine mixture separately to a moisture content of 8%;
[0063] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0064] S3: Evenly spread the glue-mixed wood shavings in a mold, and perform hot pressing for 6 minutes at a temperature of 180° C. and a pressure of 5 MPa to solidify the adhesive, thereby obtaining a jasmine particleboard.
[0065] Example 4
[0066] A jasmine particleboard is made of the following raw materials: wood shavings, a jasmine mixture, a modified phenolic resin and a composite moisture-proof agent; the amount of the jasmine mixture is 14% of the mass of the wood shavings; the amount of the adhesive is 9% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 5% of the mass of the wood shavings.
[0067] The composite moisture-proofing agent is prepared from vinyl triethoxysilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 20%: nano silicon dioxide in a mass ratio of 5:3:1.
[0068] A method for preparing a jasmine particleboard comprises the following steps:
[0069] S1: drying the wood shavings and the jasmine mixture separately to a moisture content of 6%;
[0070] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0071] S3: The glue-mixed wood shavings are evenly spread in a mold, and hot-pressed for 8 minutes at a temperature of 210° C. and a pressure of 3 MPa to solidify the adhesive to obtain a jasmine particleboard.
[0072] Example 5
[0073] A jasmine particleboard is made from the following raw materials: wood shavings, a jasmine mixture, a modified urea-formaldehyde resin adhesive, and a composite moisture-proof agent; the amount of the jasmine mixture is 15% of the mass of the wood shavings; the amount of the adhesive is 11% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 5% of the mass of the wood shavings.
[0074] The composite moisture-proofing agent is prepared from methyltriethoxysilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 10%: nano-alumina in a mass ratio of 4:3:1.
[0075] A method for preparing a jasmine particleboard comprises the following steps:
[0076] S1: drying the wood shavings and the jasmine mixture separately to a moisture content of 7%;
[0077] S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings;
[0078] S3: Evenly spread the glue-mixed wood shavings in a mold, and perform hot pressing treatment for 5 minutes at a temperature of 220° C. and a pressure of 3 MPa to solidify the adhesive, thereby obtaining a jasmine particleboard.
[0079] Comparative Example 1
[0080] The method is basically the same as Example 1, except that no jasmine mixture is added to the jasmine particleboard.
[0081] Comparative Example 2
[0082] The method is basically the same as Example 1, except that no composite moisture-proof agent is used in the jasmine particleboard.
[0083] Comparative Example 3
[0084] The method is basically the same as Example 1, except that no paraffin emulsion and inorganic minerals are added to the composite moisture-proof agent.
[0085] Comparative Example 4
[0086] It is basically the same as Example 1, except that no silane moisture-proofing agent and inorganic minerals are added to the composite moisture-proofing agent.
[0087] Comparative Example 5
[0088] The method is basically the same as Example 1, except that no silane moisture-proofing agent and paraffin emulsion are added to the composite moisture-proofing agent.
[0089] Comparative Example 6
[0090] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:0.5.
[0091] Comparative Example 7
[0092] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:1.
[0093] Comparative Example 8
[0094] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:2.
[0095] Comparative Example 9
[0096] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:3.
[0097] Comparative Example 10
[0098] The composite moisture-proofing agent is prepared from alkyl trichlorosilane moisture-proofing agent: fully refined paraffin emulsion with a concentration of 15%: nano silicon dioxide in a mass ratio of 5:4:5.
[0099] 1. Jasmine chipboard aroma experiment
[0100] Prepare particleboard according to the method of Examples 1-5 and Comparative Example 1, and cut the particleboard into small samples of the same size, number the samples, wherein the samples of Examples 1-5 are numbered 1-5, and the sample of Comparative Example 1 is numbered 6. The samples are shuffled to ensure that the source of the samples cannot be identified by numbering.
[0101] Invite 5 evaluators, ensure that the evaluators do not come into contact with any items with strong odors before the experiment, and conduct the sensory evaluation in an odor-free, well-ventilated room. Only one evaluator is allowed to conduct the evaluation at a time.
[0102] Each sample was presented to the evaluators in turn, and the odor characteristics and intensity of each sample were evaluated. Whether each sample had a jasmine aroma and the intensity of the jasmine aroma were recorded on the evaluation form. The score range was 1-5, with 1 indicating no odor and 5 indicating a strong jasmine aroma.
[0103] The evaluation forms of all evaluators were collected and the summary data are shown in Table 1.
[0104] Table 1 Sensory evaluation results
[0105]
[0106] It can be seen from Table 1 that the average odor scores of Examples 1-5 are 4.6, 4.4, 4.2, 4, and 4.2, respectively, and in Examples 1-5, all evaluators believe that Examples 1-5 have the aroma of jasmine, indicating that the present invention can make the particle board have the aroma of jasmine by adding a jasmine mixture during the production process of the particle board.
[0107] 2. Jasmine particleboard moisture-proof experiment
[0108] The particleboards prepared in Examples 1-5 and Comparative Examples 2-5 were tested for 2h moisture content and 2h water absorption thickness expansion rate according to the method of GB / T 17657-2022 Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels, and the results were recorded as shown in Table 2.
[0109] Table 2 2h moisture content and 2h water absorption thickness expansion rate of jasmine particleboard
[0110] project Moisture content (%) Water absorption thickness expansion rate (%) Example 1 4.2 5.4 Example 2 4.8 5.7 Example 3 5.1 6.3 Example 4 4.6 6.1 Example 5 5.0 5.8 Comparative Example 2 10.8 13.2 Comparative Example 3 8.4 11 Comparative Example 4 9 11.8 Comparative Example 5 9.5 12.2
[0111] It can be seen from Table 2 that:
[0112] 1. The particleboards prepared in Examples 1-5 of the present invention have 2h moisture contents of 4.2%, 4.8%, 5.1%, 4.6% and 5.0%, respectively, and 2h water absorption thickness expansion rates of 5.4%, 5.7%, 6.3%, 6.1% and 5.8%, respectively. Among them, the 2h moisture content and 2h water absorption thickness expansion rate of Example 1 are the lowest, reaching 4.2% and 5.4%, respectively. This shows that the jasmine particleboard obtained by the present invention can significantly reduce the phenomenon that the jasmine mixture has strong hygroscopicity, thereby reducing the hygroscopicity of the particleboard and significantly improving the moisture-proof performance of the particleboard.
[0113] 2. For Comparative Example 2 which does not use the composite moisture-proofing agent of the present invention, and Comparative Examples 3-5 which do not fully use the composite moisture-proofing agent of the present invention, the 2h moisture contents are 10.8%, 8.4%, 9%, and 9.5%, respectively, and the 2h water absorption thickness expansion rates are 13.2%, 11%, 11.8%, and 12.2%, respectively, which are all inferior to Examples 1-5 of the present invention. This shows that in the composite moisture-proofing agent of the present application, the silane moisture-proofing agent, paraffin emulsion, and inorganic minerals are used together to synergistically enhance the effectiveness and significantly improve the moisture-proof performance of the particleboard.
[0114] This is because: Silane moisture-proofing agents react with hydroxyl groups in cellulose and hemicellulose to form silicon-oxygen bonds, forming a stable hydrophobic layer on the fiber surface, preventing water molecules from combining with cellulose and hemicellulose, thereby reducing hygroscopicity. Paraffin wax emulsion reduces the adsorption and retention of water by forming a hydrophobic film on the fiber surface. Paraffin molecules can cover cell fibers and porous structures to prevent water from entering the fiber interior. Nano-alumina has an extremely high surface area and adsorption capacity, and can be combined with silane moisture-proofing agents and paraffin wax emulsions to enhance their adhesion and stability on the fiber surface. The addition of nano-alumina can improve the dispersibility and uniformity of moisture-proofing agents, thereby enhancing the overall moisture-proofing effect. Therefore, silane moisture-proofing agents and paraffin wax emulsions can form a double hydrophobic protective layer on the fiber surface to enhance the moisture-proofing effect. Silane moisture-proofing agents improve the hydrophobicity of fibers through chemical bonding, paraffin wax emulsions prevent water penetration by forming a physical barrier, and nano-alumina improves the adhesion and stability of moisture-proofing agents. The three can be used together to synergistically enhance the effect and significantly reduce hygroscopicity.
[0115] 3. Mechanical properties experiment of jasmine particleboard
[0116] The particleboards prepared in Example 1 and Comparative Examples 5-13 were tested for static bending strength and elastic modulus according to the method of “GB / T 17657-2022 Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels”, and the data were recorded as shown in Table 3.
[0117] Table 3 Mechanical properties of jasmine particleboard
[0118] project Static bending strength / MPa Elastic modulus / MPa Comparative Example 1 39 4121 Comparative Example 5 20 2456 Comparative Example 6 22 2512 Example 1 37 3764 Comparative Example 7 34 3376 Comparative Example 8 31 3176 Comparative Example 9 26 2834 Comparative Example 10 25 2732
[0119] From Table 3 we can see that:
[0120] 1. The jasmine particleboard prepared in the present application has a static bending strength of 37 MPa and an elastic modulus of 3764 MPa. Compared with the particleboard without the jasmine mixture, the static bending strength is only reduced by 5.1%, and the elastic modulus is only reduced by 8.7%, indicating that the particleboard of the present application still has excellent mechanical properties after adding the jasmine mixture.
[0121] This is because: nano-silica can not only improve the moisture-proof performance of the composite moisture-proof agent, but also fill the pores inside and between the fibers, reduce defects in the material, and thus improve the strength and stiffness of the fibers. At the same time, nano-silica particles can form a uniform coating on the fiber surface, increase the interfacial bonding force between the fiber and the matrix, thereby improving the strength and stiffness of the fiber, thereby reducing the impact of the weak strength of jasmine fiber on the mechanical properties of the particleboard, and improving the mechanical properties of the jasmine particleboard.
[0122] 2. In the composite moisture-proofing agent of the present application, when the ratio of silane moisture-proofing agent: paraffin emulsion: nano-silicon dioxide is selected to be 5:4:2, it has the highest mechanical properties compared with comparative example 5 in which nano-silicon dioxide is not added, and nano-silicon dioxide with different addition amounts.
[0123] This is due to: when the addition amount of nano silicon dioxide is insufficient, the particles cannot fully fill the pores inside the fiber and between the fibers, resulting in the defects in the material being unable to be effectively reduced, and the addition amount is insufficient, the coating formed by the nano silicon dioxide particles on the fiber surface is thin, the interface bonding force is insufficient, and the bonding force between the fiber and the matrix cannot be improved, so that the effect of improving strength and rigidity is limited. When the addition amount of nano silicon dioxide is too large, the particles are prone to agglomeration, forming larger particle groups, resulting in uneven dispersion, and new defects will be formed in the material instead, thereby reducing the strength and rigidity of the fiber, resulting in a decrease in the mechanical properties of the jasmine particleboard. Therefore, the present application is selected under the ratio of embodiment 1, so that the jasmine particleboard can obtain the best mechanical properties.
[0124] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A jasmine particle board, It is characterized in that The invention comprises the following raw materials: wood shavings, jasmine mixture, adhesive and composite moisture-proof agent; the amount of the jasmine mixture is 14%-16% of the mass of the wood shavings; the amount of the adhesive is 8%-12% of the mass of the wood shavings; and the amount of the composite moisture-proof agent is 3%-6% of the mass of the wood shavings.
2. A jasmine particleboard according to claim 1, Features: The jasmine flower mixture is a mixture obtained by crushing and mixing stems, stalks, leaves and flowers of jasmine flowers.
3. The jasmine particleboard according to claim 1, Features: The adhesive is one of modified phenolic resin and modified urea-formaldehyde resin.
4. A jasmine particleboard according to claim 4, Features: The composite moisture-proofing agent is prepared from silane moisture-proofing agent: paraffin emulsion: inorganic mineral matter in a mass ratio of 4-5:3-4:1-2.
5. A jasmine particleboard according to claim 4, Features: The silane moisture-proofing agent is one of methyltriethoxysilane, alkyltrichlorosilane and vinyltriethoxysilane.
6. The jasmine particleboard according to claim 4, Features: The paraffin in the paraffin emulsion is fully refined paraffin, and the concentration of the paraffin emulsion is 10-20%.
7. The jasmine particleboard according to claim 4, Features: The inorganic mineral is one of nano silicon dioxide and nano aluminum oxide.
8. A method for preparing a jasmine particleboard according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1: drying the wood shavings and the jasmine mixture to a certain moisture content respectively; S2: Mixing and stirring the dried wood shavings and the jasmine mixture, adding a moisture-proof agent during the stirring process, adding a glue after mixing evenly, and continuing to mix evenly to obtain glue-mixed shavings; S3: Evenly spread the glue-mixed wood shavings in a mold, perform heat-pressing treatment, solidify the adhesive, and obtain a jasmine particleboard.
9. The method for preparing a jasmine particleboard according to claim 8, Features: In the step S1, the mixture of wood shavings and jasmine flowers is dried to a moisture content of 5-8%.
10. The method for preparing a jasmine particleboard according to claim 8, Features: In step S3, the temperature of the hot pressing treatment is 180-220° C., the pressure is 3-5 MPa, and the treatment time is 5-10 min.
Citation Information
Patent Citations
Preparation method of artificial board containing tea, tea extracts or tea products waste
CN101596734A
Solid wood composite floor with flower and plant patterns and fragrance and preparation method thereof
CN102756412A
Process for preparing environment-friendly composite medium-density fiberboard with tea wastes
CN103102709A
Wood fiber with jasmine flower fragrance and manufacturing method thereof
CN104277470A
Fragrant health maintenance manmade fiber board and preparing method thereof
CN110802709A