Processing method of hot stamping resin wafer level lens

Through the hot embossing resin process, the metal mold is combined with the liquid resin to solve the problems of limited structure and high cost in the nanoimprinting and glass molding processes, and realize a large-area resin wafer-level lens with high precision and low fluctuation. production, improving the quality and stability of the lens.

CN118809907AActive Publication Date: 2024-10-22华天慧创科技(西安)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977057.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-22
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

In the existing wafer-level lens production process, nanoimprinting has a limited structure due to the presence of a glass substrate, and the lens surface contour accuracy and sagittal height fluctuate greatly. The glass molding process is costly and has strict equipment requirements, making it impossible to produce large-area lenses.

Method used

The hot embossing resin process is used to prepare wafer-level lenses by clamping metal molds with liquid resin. By controlling the mold contour curve accuracy and mold closing alignment accuracy, high-precision resin lens production is achieved, avoiding the limitations of the glass substrate and reducing the cost. Requirements for molds and equipment.

Benefits of technology

It achieves high precision, low fluctuation, uniform thickness and high transparency of resin wafer-level lenses, reduces production costs, can produce large-area lenses, and improves the quality and stability of the lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809907A_ABST
    Figure CN118809907A_ABST
Patent Text Reader

Abstract

The invention provides a processing method of a hot stamping resin wafer-level lens, and particularly relates to the technical field of wafer-level lens processing. The invention provides a processing method of a hot stamping resin wafer-level lens, which comprises the following steps of: coating liquid resin on a metal lower mold, closing a metal upper mold and the metal lower mold, stopping mold closing when the vertical distance between the metal upper mold and the metal lower mold reaches the thickness of the lens, thermally curing, and demolding to obtain the resin wafer-level lens, the viscosity of the liquid resin is gt; the refractive index is 1.5 to 1.9 after the epoxy resin is cured; the contour curve precision of the metal lower die and the metal upper die is independently 1t; 0.5 [mu] m; the upper metal die and the lower metal die are in a parallel state after die assembly, and the parallelism difference is smaller than or equal to 3 micrometers. According to the method provided by the invention, a working mold is not needed as a substrate, and wafer-level lenses with different structures can be obtained by using a metal mold, so that different design requirements are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wafer-level lens processing, and in particular relates to a processing method of a hot-embossed resin wafer-level lens. Background Art

[0002] At present, the common production processes of wafer-level lenses include nanoimprinting (UV-cured cold imprinting) and wafer-level glass molding (WLG). Nanoimprinting requires processing on a wafer-level glass substrate, and the presence of a glass substrate makes it impossible to design some lens structures with recurves (such as Figure 1 As shown in the figure, some structures of optical design are limited. In addition, the working molds used in nanoimprinting are all soft films, which leads to large fluctuations in the actual lens surface profile accuracy (PV), sagittal height and other data, large differences between the center and the edge, focus shift, and unstable lens quality. The PV fluctuation of the lens currently obtained is 1.5μm, and the height loss fluctuation is 1μm. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a method for processing a hot-embossed resin wafer-level lens. The lens profile curve accuracy and sag fluctuation of the lens produced by the present invention are small, and the structure is multi-dimensional.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] The present invention provides a method for processing a hot-embossed resin wafer-level lens, comprising the following steps:

[0006] Liquid resin is coated on the metal lower mold, and the metal upper mold and the metal lower mold are molded together. When the vertical distance between the metal upper mold and the metal lower mold reaches the thickness of the lens, the mold is stopped, and heat curing and demolding are performed to obtain a resin wafer-level lens;

[0007] The viscosity of the liquid resin is >400 mPa·s, and the refractive index after curing is 1.5 to 1.9;

[0008] The profile curve accuracy of the metal lower mold and the metal upper mold is independently <0.5μm;

[0009] After the mold is closed, the metal upper mold and the metal lower mold are in a parallel state, and the parallelism error is ≤3μm.

[0010] Preferably, the metal upper mold and the metal lower mold are made of nickel-phosphorus alloy.

[0011] Preferably, the mold clamping pressure is 100-500N.

[0012] Preferably, the thickness of the metal upper mold and the metal lower mold is independently 15 to 25 mm.

[0013] Preferably, the metal upper mold and the metal lower mold are independently a concave lens metal mold, a convex lens metal mold or a plane mirror metal mold.

[0014] Preferably, when the metal mold is a concave lens metal mold, the maximum depth of the concave lens metal mold is less than 1 / 10 of the thickness of the concave lens metal mold.

[0015] Preferably, before the mold is used, the surfaces of the metal upper mold and the metal lower mold are first subjected to an anti-stick deposition treatment, and after the anti-stick deposition treatment, the water drop angle on the surfaces of the metal upper mold and the metal lower mold is greater than 95°.

[0016] Preferably, the shrinkage of the liquid resin when changing from liquid to solid is greater than 0.5%, the temperature when melting is less than 200° C., the roughness after curing is less than 10 nm, the visible light transmittance is greater than 90%, and the haze is less than 0.5%.

[0017] Preferably, the liquid resin, after solidification, can withstand the impact force of a steel ball weighing ≥30g falling from 2 meters.

[0018] Preferably, the liquid resin includes liquid hot resin or molten resin.

[0019] The present invention provides a processing method for a hot-stamped resin wafer-level lens, comprising the following steps: coating a liquid resin on a metal lower mold, closing a metal upper mold with a metal lower mold, stopping closing the mold when the vertical distance between the metal upper mold and the metal lower mold reaches the thickness of the lens, thermally curing, demolding, and obtaining a resin wafer-level lens; the viscosity of the liquid resin is >400mpa·s, and the refractive index after curing is 1.5-1.9; the contour curve accuracy of the metal lower mold and the metal upper mold is independently <0.5μm; after closing the mold, the metal upper mold and the metal lower mold are in a parallel state, and the parallelism difference is ≤3μm. The method provided by the present invention does not require a working mold as a substrate, and a wafer-level lens can be obtained only by using a metal mold; a wafer-level lens of different structures can be obtained by combining metal molds with different curved surfaces, including a reverse-curved wafer-level lens, so that it can meet various different structural designs; the liquid resin is directly hot-pressed by using a metal mold, and by controlling the contour curve accuracy of the upper and lower metal molds and the alignment accuracy after closing the mold, the obtained resin lens has a high contour curve accuracy, small sag fluctuation, a smooth surface, and uniform thickness.

[0020] Furthermore, compared with the existing wafer-level glass molding (WLG) process, molten glass is used as the lens raw material, which has higher requirements for the mold, the material needs to be tungsten steel, the processing cost is high, and when the molten glass is molded, the precision and pressure requirements of the molding equipment are high, resulting in the wafer-level glass lens molding process can only operate 4-inch wafers, and large-area wafer-level lenses cannot be made, and the obtained lens is heavy; the present invention uses liquid resin as a raw material to prepare wafer lenses, and the pressure in the mold closing process is much smaller than the pressure used for wafer-level glass molding, and the requirements for molds and molding equipment are relatively small, and 8-inch resin wafer lenses with a diameter of 200mm can be made, which are light in weight. In addition, the metal mold used in the present invention is a nickel-phosphorus alloy, and its cost and processing difficulty are much lower than those of tungsten steel molds. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0022] Figure 1 It is a nano-imprint lens structure and a recurved lens structure;

[0023] Figure 2 This is a flow chart of the processing method of the hot-embossed resin wafer-level lens and lens assembly provided by the present invention. DETAILED DESCRIPTION

[0024] The present invention provides a method for processing a hot-embossed resin wafer-level lens, comprising the following steps:

[0025] Liquid resin is coated on the metal lower mold, and the metal upper mold and the metal lower mold are molded together. When the vertical distance between the metal upper mold and the metal lower mold reaches the thickness of the lens, the mold is stopped, and heat curing and demolding are performed to obtain a resin wafer-level lens;

[0026] The viscosity of the liquid resin is >400 mPa·s, and the refractive index after curing is 1.5 to 1.9;

[0027] The profile curve accuracy of the metal lower mold and the metal upper mold is independently <0.5μm;

[0028] After the mold is closed, the metal upper mold and the metal lower mold are in a parallel state, and the parallelism difference is ≤3μm.

[0029] In the present invention, the profile accuracy of the metal upper mold and the metal lower mold is independently <0.5 μm, preferably <0.4 μm. The small profile accuracy of the metal mold is conducive to improving the profile accuracy of the resin lens.

[0030] In the present invention, the material of the metal upper mold and the metal lower mold is preferably nickel-phosphorus alloy, and the thickness of the metal upper mold and the metal lower mold is preferably 15 to 25 mm, more preferably 18 to 22 mm, independently.

[0031] In the present invention, the metal upper mold and the metal lower mold are independently preferably a concave lens metal mold, a convex lens metal mold or a plane mirror metal mold. The metal mold structure can be processed and manufactured according to the product lens design structure to meet various different structural designs. When the metal mold is a concave lens metal mold, the maximum depth of the concave lens metal mold is preferably less than 1 / 10 of the thickness of the concave lens metal mold. By limiting the maximum depth of the concave surface in the concave lens metal mold, the concave lens metal mold is prevented from being deformed due to force during the metal mold closing process.

[0032] In the present invention, before the mold is used, it is preferred to first perform an anti-adhesion deposition treatment on the surface of the metal upper mold and the metal lower mold. The present invention has no special requirements for the anti-adhesion deposition treatment, and conventional technical means in the art can be used. The present invention specifically uses a surface-coated waterproof film. Anti-adhesion deposition is performed on the mold surface to reduce the surface energy of the metal mold, and the water drop angle is >95°.

[0033] In the present invention, the liquid resin preferably includes a room temperature liquid resin or a molten resin, the viscosity of the liquid resin is >400 mpa·s, the refractive index after curing is 1.5-1.9, the shrinkage rate of the liquid resin when changing from liquid to solid is preferably >0.5%, the temperature when melting is preferably <200°C, the roughness after curing is preferably <10nm, the visible light transmittance is preferably >90%, and the haze is preferably <0.5%. In the present invention, the liquid resin after curing can preferably withstand the impact force of a steel ball of ≥30g falling at 2 meters.

[0034] There is no special requirement for the coating method in the present invention, and conventional coating methods in the art can be used.

[0035] In the present invention, the mold clamping pressure is preferably 100 to 500 N, more preferably 200 to 450 N. Using liquid resin as a raw material for preparing the lens can reduce the mold clamping pressure.

[0036] In the present invention, after the mold is closed, the metal upper mold and the metal lower mold are in a parallel state, and the parallelism difference is ≤3μm, preferably ≤2.5μm. The present invention can reduce the height loss fluctuation of the obtained lens, reduce the difference between the center and the edge, and ensure the uniformity of the thickness of the obtained lens by controlling the parallelism difference.

[0037] In the present invention, the temperature of the thermal curing is preferably 110-130° C., preferably 120° C., and the time is preferably 5-20 min, more preferably 10-15 min. In the present invention, the thermal curing is preferably achieved by heating the mold.

[0038] The present invention has no special requirements for the demoulding method, and the commonly used technical means in the field can be used. In a specific embodiment of the present invention, the mold group after heat curing is placed on a separation device, and the metal upper mold is lifted by the separation device to separate the two metal molds. A flat-mouth nitrogen dust-free air gun with a pressure of 10kPa is used to blow along the contact edge gap between the lens and the metal mold to separate the lens from the metal mold. If the blowing cannot separate them, a tool is placed between the lens and the metal mold, and then the air is blown. It should be noted that when using the tool, it is necessary to avoid damaging the metal mold to reduce the service life of the metal mold.

[0039] In the present invention, the resin wafer-level lens obtained by the above method is a single-layer structure (referred to as the first single-layer lens). A person skilled in the art can prepare another single-layer structure lens (referred to as the second single-layer lens) according to the above method, and then combine the first single-layer lens with the second single-layer lens to obtain a lens group.

[0040] Combine the following Figure 2 The processing method of the resin wafer-level lens and lens assembly of the present invention is further explained.

[0041] like Figure 2 As shown, 1-concave metal mold, 2-concave metal mold, 3-liquid resin, 4-convex metal mold, 5-reverse curved structure lens, 6-convex structure lens, 7-lens group with array structure, 8-single lens group.

[0042] The present invention coats liquid resin 3 on the surface of a convex metal mold 4 (i.e., a metal lower mold), and molds it with a convex metal mold (not numbered in the figure), and obtains an inversely curved structure lens 5 after curing and demolding; coats liquid resin 3 on the surface of a concave metal mold 2 (i.e., a metal lower mold), and molds it with a concave metal mold 1 (i.e., a metal upper mold), and obtains a convex structure lens 6 after curing and demolding; the inversely curved structure lens 5 and the convex structure lens 6 are aligned and combined, and then bonded to obtain a lens group 7 with an array structure, and the lens group 7 is cut to obtain a single lens group 8.

[0043] In the present invention, the alignment accuracy is preferably ≤3 μm. The present invention has no special requirements for the bonding, and conventional technical solutions in the art can be used, such as glue bonding, laser welding, etc. In the present invention, the thickness of the bonding layer is preferably 3 μm.

[0044] The present invention has no special requirements for the cutting method, and the cutting method commonly used in the art can be used. In the present invention, the chipping after cutting is preferably ≤15 μm.

[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.

[0046] Example 1

[0047] The contour curve accuracy of the convex metal lower die used in this embodiment is 0.05 μm, and the material is nickel-phosphorus alloy; the contour curve accuracy of the concave metal upper die used is 0.04 μm, and the material is nickel-phosphorus alloy;

[0048] A liquid resin with a viscosity of 580 MPa·s, a refractive index of 1.5 after curing, a visible light transmittance of 92%, and a haze of 0.48% is applied to the convex metal lower mold, and the concave metal upper mold and the convex metal lower mold are molded together with a mold clamping pressure of 500 N. The concave metal upper mold and the convex metal lower mold are kept in a parallel state. The mold clamping is stopped when the vertical distance between the concave metal upper mold and the convex metal lower mold reaches the required thickness. The parallelism difference between the upper and lower molds is controlled to be ±3 μm. The combined mold is placed in an oven for heating, and demolding is performed after 120°C for 10 minutes to obtain a reverse curved resin wafer-level lens. The resin wafer size is 200 mm in diameter and 0.7 mm in thickness. The small lens size has a sagittal height of 73 μm and an aperture size of 213 μm.

[0049] Three wafer-level lenses were processed through this process, and the profile of one of the curved surfaces of the three wafer-level lenses was measured using UA3P. The collected data is shown in Table 1:

[0050] Table 1 Test results of the precision and vector height of the resin wafer-level lens

[0051] Film number Sheet 1 Sheet 2 Slice 3 Surface accuracy / PV 0.4μm 0.32μm 0.36μm Lens height / SAG 0.0731mm 0.0734mm 0.0735mm

[0052] As can be seen from Table 1, the lenses continuously manufactured by this process have a surface accuracy fluctuation of 0.04μm between pieces and a sagittal height fluctuation of 0.0004mm between pieces. Their stability is better than that of the lenses manufactured by nanoimprinting process, and the problem of large fluctuation between nanoimprinting pieces can be solved.

[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for processing a hot-embossed resin wafer-level lens, characterized in that: The following steps are involved: Liquid resin is coated on the metal lower mold, and the metal upper mold and the metal lower mold are molded together. When the vertical distance between the metal upper mold and the metal lower mold reaches the thickness of the lens, the mold is stopped, and heat curing and demolding are performed to obtain a resin wafer-level lens; The viscosity of the liquid resin is >400 mPa·s, and the refractive index after curing is 1.5 to 1.9; The profile curve accuracy of the metal lower mold and the metal upper mold is independently <0.5μm; After the mold is closed, the metal upper mold and the metal lower mold are in a parallel state, and the parallelism error is ≤3μm.

2. The processing method according to claim 1, characterized in that: The material of the metal upper mold and the metal lower mold is nickel-phosphorus alloy.

3. The processing method according to claim 1, characterized in that: The mold clamping pressure is 100-500N.

4. The processing method according to claim 1 or 2, characterized in that: The thickness of the metal upper mold and the metal lower mold is independently 15 to 25 mm.

5. The processing method according to claim 1, characterized in that: The metal upper mold and the metal lower mold are independently a concave lens metal mold, a convex lens metal mold or a plane mirror metal mold.

6. The processing method according to claim 5, characterized in that: When the metal mold is a concave lens metal mold, the maximum depth of the concave lens metal mold is less than 1 / 10 of the thickness of the concave lens metal mold.

7. The processing method according to claim 1 or 2, characterized in that: Before using the mold, the surfaces of the metal upper mold and the metal lower mold are first subjected to anti-stick deposition treatment. After the anti-stick deposition treatment, the water drop angles on the surfaces of the metal upper mold and the metal lower mold are greater than 95°.

8. The processing method according to claim 1, characterized in that: The shrinkage rate of the liquid resin when changing from liquid to solid is greater than 0.5%, the temperature when melting is less than 200° C., the roughness after curing is less than 10 nm, the visible light transmittance is greater than 90%, and the haze is less than 0.5%.

9. The processing method according to claim 1, characterized in that: After being cured, the liquid resin can withstand the impact force of a steel ball weighing ≥30 g falling from a height of 2 meters.

10. The processing method according to claim 1, 8 or 9, characterized in that: The liquid resin includes room temperature liquid resin or molten resin.