Ferroelastic body material domain overturning path and loading and unloading characteristic prediction method
The spontaneous strain process of ferroelastic materials is calculated through density functional theory, a strain unit cell is constructed and the stress-strain curve is drawn, which solves the problem in the existing technology that the domain flip path and critical load of ferroelastic materials are difficult to obtain, and realizes the increase of ferroelasticity. Efficient application of toughness mechanism in high-temperature ceramic coatings.
Patent Information
- Application Number
- CN202410916309.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-09
AI Technical Summary
It is difficult to obtain the domain flipping path and critical load of ferroelastic materials at the same time with the existing technology, resulting in low application efficiency of ferroelastic toughening mechanism in high-temperature ceramic coatings, and experimental methods and theoretical calculation methods have high cost, low efficiency and inaccurate results. problem.
Density functional theory is used to calculate the spontaneous strain process of ferroelastomer materials under external mechanical loads, construct unit cells with different strains, optimize the geometric structure, draw stress-strain curves, and obtain the atomic migration process and criticality of domain flipping. mechanical loads.
The accuracy and efficiency of predicting the ferroelastic domain flip path and loading and unloading characteristics are achieved, the cost is reduced, and the application efficiency of the ferroelastic toughening mechanism in high-temperature ceramic coatings is improved.
Smart Images

Figure CN118824433A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ferroelastic materials, and in particular to a method for predicting domain flipping paths and loading and unloading characteristics of ferroelastic materials. Background Art
[0002] Ferroelastic toughening is a property unique to ferroelastics. Under stress, some regions that are oriented according to stress orientation will spontaneously form inside the ferroelastic grains, also known as ferroelastic domains. The rotation of these ferroelastic domains will absorb part of the energy of crack propagation, resulting in stress-strain hysteresis in the material, thereby significantly improving the fracture toughness of the material. Therefore, ferroelastic toughening provides structural stability for the application of materials and devices. It is particularly noteworthy that ferroelasticity is a rare toughening mechanism suitable for high-temperature environments, so it is also widely used in the field of high-temperature ceramic coatings.
[0003] In the thermal barrier coatings of high-performance aircraft engines, the high-temperature brittleness of ceramic materials is an important factor leading to coating spalling failure. By introducing the ferroelastic toughening mechanism, the fracture toughness of the ceramic coating can be effectively improved, thereby extending its service life. Therefore, yttria-stabilized zirconia (YSZ) materials with excellent ferroelastic toughening properties are also the only coating materials currently being applied. In addition, some new thermal barrier coating materials have also been found to have excellent ferroelastic toughening properties, such as rare earth tantalates (RETaO4), rare earth aluminates (REAlO3) and their modified materials.
[0004] At present, the research on ferroelastic domain reversal is mainly divided into experimental methods and theoretical calculation methods. In terms of experimental methods, the existing technologies mainly include in-situ transmission electron microscopy loading method and indentation method, and the theoretical calculation methods mainly include phase field method and transition state calculation method.
[0005] 1) In-situ transmission electron microscopy loading method: Professor Gao Peng of Peking University used in-situ transmission electron microscopy to experimentally confirm that PbTiO3 can be loaded under compressive stress. c → a domain transition, and as the mechanical load continues to increase, the newly generated a The domains will run through the entire film and continue to "grow". However, in-situ transmission electron microscopy requires the transmission electron microscope to be equipped with an in-situ nanomechanical testing device, and the requirements for preparing the samples to be tested are high and expensive.
[0006] 2) Indentation method: Professor Zhou Yichun of Xiangtan University observed a 90% crack tip on the surface of yttria-stabilized zirconium oxide single crystal epitaxial film by Vickers indentation. o The ferroelastic domains are arranged in the single crystal film. It is speculated that the external force in the indentation area may cause some c Domain transformation aThe transformation of the domain structure helps to prevent the further expansion of the crack, thereby achieving the purpose of toughening. However, the indentation method can only observe the final morphology of the domain structure in a non-in-situ form near the crack tip of the ferroelastic material, and cannot obtain the process of domain reversal, nor can it accurately measure the critical load of domain reversal.
[0007] 3) Phase field method: Professor Luo Jun of Huazhong University of Science and Technology used the phase field method to define variants of different crystallographic orientations as order parameters. Based on the conservation of volume and energy during domain reversal, he studied the crack propagation process in tetragonal yttria-stabilized zirconia single crystals under different external loads from a theoretical level, revealing the influence of crystal orientation and loading type on domain reversal. Although the phase field method can study a larger material system than the density functional theory method, it is necessary to experimentally measure the coercive force of domain reversal, and then use this to set the energy barrier for domain reversal during the phase field simulation. This simulation method cannot obtain the stress-strain curve of ferroelastic materials, so additional experimental data (coercive force) is required to assist in modeling, which is inefficient.
[0008] 4) Transition state calculation method: Professor Jinsong Huang of the University of North Carolina used density functional theory to calculate the mutual domain reversal process of two oriented domains in two-dimensional inorganic-organic hybrid perovskite by searching for transition states, and theoretically predicted that its ferroelasticity originates from the inorganic octahedral distortion caused by the rotation of non-spherical methylammonium cations; although the transition state calculation can accurately obtain the change in the total energy of the system in any intermediate state, it cannot obtain the stress-strain curve of the material, nor can it give the critical mechanical load for domain reversal. In addition, the transition state calculation requires the variant structure before / after the domain reversal, so the domain reversal path obtained is related to the domain orientation given in advance, and the result has a certain degree of randomness, so there may be deviations between the predicted results and the actual results.
[0009] The above methods all have limitations. Therefore, the present invention reports a simpler method for predicting the domain reversal path and loading and unloading characteristics of ferroelastic materials, which can provide theoretical guidance for the design and development of high-performance materials, devices, and coatings. Summary of the invention
[0010] In view of the deficiencies in the above-mentioned background technology, the present invention mainly solves the problem that the domain reversal path and critical load of ferroelastic materials are difficult to obtain simultaneously. The present invention provides a method for predicting the domain reversal path and loading and unloading characteristics of ferroelastic materials. The method is based on density functional theory. By calculating the ferroelastic material under an external mechanical load, the process of spontaneous strain transformation in the crystal is studied. The size and direction of the mechanical load used are controllable. Not only can the atomic migration process of ferroelastic domain reversal be obtained, but also the critical mechanical load of domain reversal and the stress-strain curve of the material can be accurately obtained.
[0011] The first object of the present invention is to provide a method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials, comprising the following steps: Obtaining the spontaneous strain orientation of ferroelastic materials; According to the spontaneous strain orientation of the ferroelastic material, unit cells with different compressive or tensile strains are sequentially constructed along the tensile or compressive strain direction; Density functional theory was used to optimize the geometry of each unit cell to obtain a stable configuration; A ball-and-stick model was drawn based on the stable configuration and arranged from small to large strains to obtain the atomic migration process of domain flipping. The stress corresponding to each stable configuration under different strain conditions is extracted in turn, and the stress-strain curve of the ferroelastic material is plotted to obtain the critical mechanical load for domain reversal.
[0012] Preferably, the critical mechanical load for domain reversal is the stress corresponding to the first peak of the stress-strain curve deviating from the linear region.
[0013] Preferably, the ferroelastic material includes YTaO4, YSZ, BaTiO3, LaNbO4, BiFeO3, WO3 or a two-dimensional inorganic-organic hybrid perovskite.
[0014] Preferably, the spontaneous strain orientation of the ferroelastic material is obtained according to the crystal symmetry of the ferroelastic material.
[0015] Preferably, the strain of the constructed unit cell is consistent with the spontaneous strain orientation of the ferroelastic material, and the strain value ranges from ±0 to 50%.
[0016] Preferably, the strain interval of each unit cell is less than 2%.
[0017] Preferably, when the geometric structure of each unit cell is optimized, only the unit cell size in the spontaneous strain direction is fixed.
[0018] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for predicting the domain reversal path and loading and unloading characteristics of a ferroelastic material. The method determines the spontaneous strain orientation of the ferroelastic material based on the crystal symmetry of the ferroelastic material, and constructs unit cells with different compression / tensile strains along the tensile / compression strain direction. The density functional theory method is used to effectively predict the domain reversal path and loading and unloading characteristics of the ferroelastic material. The atomic migration process of the domain reversal can be obtained based on the stable configuration. The stress-strain curve of the material can be accurately drawn, and the critical mechanical load of the domain reversal can be obtained.
[0019] The present invention is based on density functional theory. By calculating the spontaneous strain transformation process of ferroelastic materials under external mechanical load, the size and direction of the mechanical load used can be controlled. Not only can the atomic migration process of ferroelastic domain reversal be obtained, but also the critical mechanical load of domain reversal and the stress-strain curve of the material can be accurately obtained. Compared with experimental methods such as in-situ transmission electron microscopy and indentation method, the calculation method of the present invention has low cost and high efficiency; compared with the phase field method, the method of the present invention can accurately obtain the critical mechanical load of domain reversal and the stress-strain curve of the material; compared with transition state calculation, the method of the present invention does not need to give two variants before / after domain reversal at the same time, which is simpler and more convenient, and can accurately predict the stress-strain curve of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 1 is a ball-and-stick model diagram of the YTaO4 crystal in Example 1, (a) a schematic diagram of applying tensile strain along the
[001] direction, and (b) a schematic diagram of applying compressive strain along the
[100] direction; Figure 2 is the stress-strain curve of the YTaO4 crystal in Example 1 in the tensile state along the
[001] direction; Figure 3 is a diagram of the ferroelastic domain reversal process of the YTaO4 crystal in the stretched state along the
[001] direction in Example 1; Figure 4 is the stress-strain curve of the YTaO4 crystal in the compression state along the
[100] direction in Example 1; Figure 5 is a diagram of the ferroelastic domain reversal process of the YTaO4 crystal in the compressed state along the
[100] direction in Example 1; Figure 6 1 is a model diagram of the stretching process of LaNbO4 crystal in Example 2, (a) is a schematic diagram of applying tensile strain along the
[001] direction, and (b) is a stress-strain curve of the LaNbO4 crystal in the stretching state along the
[100] direction; Figure 7 is a diagram of the ferroelastic domain reversal process of the LaNbO4 crystal in the stretched state along the
[001] direction in Example 2; Figure 8 1 is a model diagram of the stretching process of BaTiO3 crystal in Example 3, (a) is a schematic diagram of applying tensile strain along the
[100] direction, and (b) is a stress-strain curve of the BaTiO3 crystal in the stretched state along the
[100] direction; Fig. 9 This is a diagram of the ferroelastic domain reversal process of the BaTiO3 crystal in Example 3 when stretched along the
[100] direction. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0022] The main purpose of the present invention is to study the process of spontaneous strain transformation in the crystal of ferroelastic materials under external mechanical loads based on density functional theory. The size and direction of the mechanical load used are controllable, which can not only obtain the atomic migration process of ferroelastic domain reversal, but also accurately obtain the critical mechanical load of domain reversal and the stress-strain curve of the material.
[0023] In order to achieve the above object, the present invention provides a method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials, comprising the following steps: Obtaining the spontaneous strain orientation of ferroelastic materials; According to the spontaneous strain orientation of the ferroelastic material, unit cells with different compressive or tensile strains are sequentially constructed along the tensile or compressive strain direction; Density functional theory was used to optimize the geometry of each unit cell to obtain a stable configuration; A ball-and-stick model was drawn based on the stable configuration and arranged from small to large strains to obtain the atomic migration process of domain flipping. The stress magnitude corresponding to each stable configuration under the above-mentioned different strain conditions is extracted in turn, and the stress-strain curve of the ferroelastic material is plotted to obtain the critical mechanical load for domain reversal.
[0024] It should be noted that each stable configuration of strain has a corresponding stress.
[0025] The critical mechanical load for domain reversal is the stress corresponding to the first peak of the stress-strain curve that deviates from the linear region.
[0026] The ferroelastic material includes YTaO4, YSZ, BaTiO3, LaNbO4, BiFeO3, WO3 or a two-dimensional inorganic-organic hybrid perovskite.
[0027] The spontaneous strain orientation of the ferroelastic material is obtained according to the crystal symmetry of the ferroelastic material.
[0028] Specifically, whether the material under study has ferroelastic properties is determined based on the space group of the crystal structure, the crystal symmetry of the ferroelastic body to be studied is analyzed, and the spontaneous strain orientation of the ferroelastic body is determined.
[0029] The strain of the constructed unit cell is consistent with the spontaneous strain orientation of the ferroelastic material, and the strain value ranges from ±0 to 50%.
[0030] The strain interval of each of the unit cells is less than 2%.
[0031] When optimizing the geometry of each unit cell, only the unit cell size in the spontaneous strain direction is fixed; the other directions are not fixed. When optimizing the geometry, based on density functional theory, the atomic coordinates of the input system are adjusted to obtain a relatively stable unit cell structure.
[0032] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified.
[0033] Example 1 YTaO4 ferroelastic domain reversal path and loading and unloading characteristics prediction method, including: (1) Based on the symmetry of the crystal structure, it is determined that the monoclinic YTaO4 has ferroelastic properties. The crystal symmetry of the ferroelastic body to be studied is analyzed, and it is determined that the YTaO4 ferroelastic body has spontaneous compressive strain along the
[001] crystal direction and spontaneous tensile strain along the
[100] crystal direction.
[0034] (2) According to the characteristics of spontaneous strain, unit cells with different tensile strains are constructed sequentially along the
[001] crystal direction; or unit cells with different compressive strains are constructed sequentially along the
[100] crystal direction.
[0035] (3) Density functional theory is used to optimize the geometric structure of the above series of unit cells to obtain the final stable configuration.
[0036] (4) Draw the ball-and-stick models of the stable configurations of YTaO4 under different strain states and arrange them from small to large strains to obtain the atomic migration process of YTaO4 domain reversal.
[0037] (5) The stress corresponding to each stable configuration under different strain conditions is extracted in turn, and the stress-strain curve of YTaO4 under tension or compression conditions is plotted respectively, so as to obtain the critical mechanical load for the flipping of the ferroelastic domain in YTaO4.
[0038] The strain value range of the unit cell constructed in step (2) is: ±30%; The strain interval of the unit cell constructed in step (2) is 1%; In the step (3), in the unit cell under tensile strain, only the unit cell size in the
[100] direction is fixed, and the other directions are not fixed; in the unit cell under compressive strain, only the unit cell size in the
[001] direction is fixed, and the other directions are not fixed; The critical mechanical load for domain reversal in step (5) is the stress corresponding to the first peak value of the stress-strain curve deviating from the linear region.
[0039] Figure 1Schematic diagram of the ball-and-stick model of the YTaO4 crystal in Example 1, (a) a schematic diagram of applying tensile strain along the
[001] direction, and (b) a schematic diagram of applying compressive strain along the
[100] direction.
[0040] Figure 2 The stress-strain curve of the YTaO4 crystal in Example 1 in the tensile state along the
[001] direction is shown in the fitting curve. The stress-strain curve deviates from the linear region when the tensile strain is 3.5%. The load corresponding to this point is the critical mechanical load for the ferroelastic domain flipping, which is 2.47 GPa. When the strain is greater than 5%, the stretching of the YTaO4 crystal is linear elastic. When the strain is greater than 30%, plastic deformation occurs, indicating that the material is about to be broken.
[0041] Figure 3 This is a diagram of the ferroelastic domain reversal process of the YTaO4 crystal in the tensile state along the
[001] direction in Example 1. As the tensile strain increases, the monoclinic YTaO4 crystal a , c The angle between the axes changes from 91.47 o becomes 87.96 o , which shows that the original direction along
[100] a domain, under the tensile load along the
[001] direction, will gradually flip to form a c Category.
[0042] Figure 4 The stress-strain curve of the YTaO4 crystal in Example 1 in the compression state along the
[100] direction is shown in the fitting curve. The stress-strain curve deviates from the linear region when the compression strain is -4.0%. The load corresponding to this point is the critical mechanical load for the ferroelastic domain flipping, which is 4.20 GPa. When the strain is greater than -6%, the compression of the YTaO4 crystal is linear elastic. When the strain is greater than -20%, plastic deformation occurs and the stress decreases rapidly, indicating that the material is crushed.
[0043] Figure 5 This is a diagram of the ferroelastic domain reversal process of the YTaO4 crystal in the compression state along the
[100] direction in Example 1. As the compressive strain increases, the monoclinic YTaO4 crystal a , c The angle between the axes changes from 91.47 o becomes 84.05 o , which shows that the original direction along
[100] a domain, under the compressive load along the
[100] direction, will gradually flip to form a domain along the
[001] direction. c Category.
[0044] Example 2 The LaNbO4 ferroelastic domain reversal path and loading and unloading characteristics prediction method includes: (1) Based on the symmetry of the crystal structure, it is determined that the monoclinic LaNbO4 phase under study has ferroelastic properties. The crystal symmetry of the ferroelastic body to be studied is analyzed, and it is determined that the LaNbO4 ferroelastic body has spontaneous compressive strain along the
[001] crystal direction.
[0045] (2) According to the characteristics of spontaneous compressive strain, unit cells with different tensile strains are constructed sequentially along the
[001] crystal direction.
[0046] (3) Density functional theory is used to optimize the geometric structure of the above series of unit cells to obtain the final stable configuration.
[0047] (4) Draw the ball-and-stick model of the stable configuration of LaNbO4 under different strain states mentioned above and arrange them from small to large strains to obtain the atomic migration process of LaNbO4 domain reversal.
[0048] (5) The stress corresponding to each stable configuration under different strain conditions is extracted in turn, and the stress-strain curve of LaNbO4 under tensile conditions is plotted to obtain the critical mechanical load for the flipping of the ferroelastic domain in LaNbO4.
[0049] The strain value range of the unit cell constructed in step (2) is: ±32%; The strain interval of the unit cell constructed in step (2) is 1%; In the step (3), only the unit cell size in the
[001] direction is fixed in the tensile strained unit cell, and the remaining directions are not fixed; The critical mechanical load for domain reversal in step (5) is the stress corresponding to the first peak value of the stress-strain curve deviating from the linear region.
[0050] Figure 6 The figure is a model diagram of the stretching process of LaNbO4 crystal in Example 2. (a) is a schematic diagram of applying tensile strain along the
[001] direction, and (b) is a stress-strain curve of the LaNbO4 crystal in the tensile state along the
[100] direction. The fitting curve shows that when the compressive strain is 8.0%, the stress-strain curve deviates from the linear region. The load corresponding to this point is the critical mechanical load for the ferroelastic domain flipping, which is 2.87 GPa. When the strain is greater than 12%, the stretching of the LaNbO4 crystal is linear elastic. When the strain is greater than 27%, plastic deformation occurs, and the stress decreases rapidly, indicating that the material is broken.
[0051] Figure 7 is a diagram of the ferroelastic domain reversal process of the LaNbO4 crystal in the tensile state along the
[001] direction in Example 2. As the tensile strain increases, the monoclinic LaNbO4 crystala , c The angle between the axes is from 93.02 o becomes 85.13 o , which shows that the original direction along
[100] a domain, under the tensile load along the
[001] direction, will gradually flip to form a c Category.
[0052] Example 3 BaTiO3 ferroelastic domain reversal path and loading and unloading characteristics prediction method, including: (1) Based on the symmetry of the crystal structure, it is determined that the tetragonal BaTiO3 phase under study has ferroelastic properties. The crystal symmetry of the ferroelastic body to be studied is analyzed, and it is determined that the BaTiO3 ferroelastic body has spontaneous tensile strain along the
[001] crystal direction.
[0053] (2) According to the characteristics of spontaneous tensile strain, unit cells with different tensile strains are constructed sequentially along the
[100] crystal direction.
[0054] (3) Density functional theory is used to optimize the geometric structure of the above series of unit cells to obtain the final stable configuration.
[0055] (4) Draw the ball-and-stick models of the stable configurations of BaTiO3 under different strain states and arrange them from small to large strains to obtain the atomic migration process of BaTiO3 domain reversal.
[0056] (5) The stress corresponding to each stable configuration under different strain conditions is extracted in turn, and the stress-strain curve of BaTiO3 under tensile conditions is plotted to obtain the critical mechanical load for the flipping of the ferroelastic domain in BaTiO3.
[0057] The strain value range of the unit cell constructed in step (2) is: ±40%; The strain interval of the unit cell constructed in step (2) is 1%; In the step (3), only the unit cell size in the
[100] direction is fixed in the tensile strained unit cell, and the remaining directions are not fixed; The critical mechanical load for domain reversal in step (5) is the stress corresponding to the first peak value of the stress-strain curve deviating from the linear region.
[0058] Figure 8The figure is a model diagram of the stretching process of BaTiO3 crystal in Example 3. (a) is a schematic diagram of applying tensile strain along the
[100] direction, and (b) is a stress-strain curve of BaTiO3 crystal in the stretching state along the
[100] direction. The fitting curve shows that when the tensile strain is 3.5%, the stress-strain curve deviates from the linear region. The load corresponding to this point is the critical mechanical load for the ferroelastic domain flipping, which is 3.62 GPa. When the strain is greater than 5%, the stretching of BaTiO3 crystal is linear elastic. When the strain is greater than 16%, plastic deformation occurs, indicating that the material is about to be broken.
[0059] Fig. 9 The diagram is a diagram of the ferroelastic domain reversal process of the BaTiO3 crystal in the tensile state along the
[100] direction in Example 3. As the tensile strain increases, the long axis of the tetragonal BaTiO3 crystal gradually turns from the
[001] direction to the
[100] direction, which indicates that the long axis of the tetragonal BaTiO3 crystal originally along the
[001] direction c domain, under the tensile load along the
[100] direction, will gradually flip to form a a Category.
[0060] The present invention describes preferred embodiments and their effects. However, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials, characterized in that: The following steps are involved: Obtaining the spontaneous strain orientation of ferroelastic materials; According to the spontaneous strain orientation of the ferroelastic material, unit cells with different compressive or tensile strains are sequentially constructed along the tensile or compressive strain direction; Density functional theory was used to optimize the geometry of each unit cell to obtain a stable configuration; A ball-and-stick model was drawn based on the stable configuration and arranged from small to large strains to obtain the atomic migration process of domain flipping. The stress magnitude corresponding to each stable configuration under different strain conditions is extracted in turn, and the stress-strain curve of the ferroelastic material is plotted to obtain the critical mechanical load for domain reversal.
2. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: The critical mechanical load for domain switching is the stress corresponding to the first peak of the stress-strain curve deviating from the linear region.
3. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: The ferroelastic material includes YTaO4, YSZ, BaTiO3, LaNbO4, BiFeO3, WO3 or a two-dimensional inorganic-organic hybrid perovskite.
4. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: The spontaneous strain orientation of the ferroelastic material is obtained according to the crystal symmetry of the ferroelastic material.
5. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: The strain of the constructed unit cell is consistent with the spontaneous strain orientation of the ferroelastic material, and the strain value ranges from ±0 to 50%.
6. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: The strain interval of each of the unit cells is less than 2%.
7. The method for predicting domain reversal path and loading and unloading characteristics of ferroelastic materials according to claim 1, characterized in that: When optimizing the geometry of each unit cell, only the unit cell size in the spontaneous strain direction is fixed.
Citation Information
Patent Citations
Phase field simulation method for domain overturning dynamics of hafnium oxide-based ferroelectric film
CN118098451A
Self-optimizing, inverse analysis method for parameter identification of nonlinear material constitutive models
US20130289953A1
Integrated process-structure-property modeling frameworks and methods for design optimization and / or performance prediction of material systems and applications of same
US20200089826A1
Methods and systems for upscaling mechanical properties of geomaterials