Secondary battery and electronic device
By using a combination of polyvinyl butyral, lithium difluorophosphate, and trinitrile compounds in secondary batteries, the problems of PVDF binder stability and environmental pollution are solved, and the shedding resistance of the positive electrode and battery performance are improved. Achieving green and sustainable battery performance improvement.
Patent Information
- Application Number
- CN202411116513.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-22
AI Technical Summary
The polyvinylidene fluoride (PVDF) binder used in existing secondary batteries can easily lead to a decrease in slurry stability and affect battery performance. Moreover, the R142B used in its preparation process is a high-risk environmental pollutant and violates green safety standards. Requirements for sustainable development.
By adding polyvinyl butyral to the positive electrode composition of the secondary battery and using lithium difluorophosphate and trinitrile compounds in the electrolyte, the resistance to shedding of the positive electrode is improved, the initial resistance is reduced, and the low-temperature rate characteristics are improved.
It significantly improves the shedding resistance and adhesion of the positive electrode, reduces the initial resistance of the secondary battery, and improves the low-temperature rate characteristics, which meets the requirements of green and sustainable development.
Smart Images

Figure BDA0004993888500000141 
Figure BDA0004993888500000142 
Figure BDA0004993888500000151
Abstract
Description
Technical Field
[0001] The present application relates to the field of energy storage, and in particular to a secondary battery and an electronic device. Background Art
[0002] Secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and have been widely used. Secondary batteries usually have battery components such as a positive electrode, a negative electrode, and a separator that separates the positive electrode from the negative electrode. An electrode (such as a positive electrode or a negative electrode) usually has a current collector and an electrode composite material layer formed on the current collector. For example, the positive electrode composite material layer is usually formed by applying a positive electrode slurry on the current collector and drying it. The positive electrode slurry is formed by containing a positive electrode active material, a conductive material for improving conductivity, and a bonding material for bonding these components in a dispersion medium. In addition, polyvinylidene fluoride (PVDF) and the like have been used as bonding materials for forming the positive electrode composite material layer. PVDF is prone to gelling, resulting in decreased slurry stability and affecting battery performance. PVDF is a fluorine-containing binder, and its polymer monomer VDF is prepared by dehydrochlorination of 1,1-difluoro-1-chloroethane (R142B). However, R142B is a highly dangerous environmental pollutant and does not meet the requirements of green and sustainable development of the new energy industry. Developed countries such as the European Union are gradually restricting its use in lithium batteries. Summary of the invention
[0003] The embodiments of the present application solve the problems existing in the prior art to some extent by adjusting the positive electrode composition and the components in the electrolyte used in the secondary battery. The inventors of the present application found that the positive electrode active material layer includes a positive electrode active material and polyvinyl butyral, and the electrolyte includes lithium difluorophosphate and a trinitrile compound, which can not only improve the positive electrode's resistance to shedding, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics, thereby completing the present application.
[0004] In some embodiments, the polyvinyl butyral has at least one of the following characteristics:
[0005] Feature 1. It has a particle shape and an average particle size of 20 microns to 100 microns;
[0006] Feature 2: The degree of acetalization is 30 mol% to 60 mol%;
[0007] Feature 3: Average molecular weight is 3×10 4 Up to 20×10 4 .
[0008] In some embodiments, the positive electrode active material layer further includes an auxiliary agent, and the auxiliary agent includes at least one of propylene glycol laurate, pentaerythritol oleate, polyethylene glycol oleate, polypropylene glycol oleate, polyoxyethylene glycerol, or polyoxypropylene glycerol.
[0009] In some embodiments, the trinitrile compound is selected from at least one of 1,2,3-propanetricarboxylate, 1,3,5-pentanetricarboxylate, 1,2,6-hexanetricarboxylate, 1,3,6-hexanetricarboxylate, 1,2,4-tris(2-cyanoethoxy)butane, 1,2,3-tris(2-cyanoethoxy)propane, 1,1,1-tris(cyanoethoxymethylene)ethane, 1,1,1-tris(cyanoethoxymethylene)propane, 3-methyl-1,3,5-tris(cyanoethoxy)pentane, 1,2,7-tris(cyanoethoxy)heptane, 1,2,6-tris(cyanoethoxy)hexane or 1,2,5-tris(cyanoethoxy)pentane.
[0010] In some embodiments, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.01 parts by mass to 1.5 parts by mass, and / or the trinitrile compound is in an amount of 0.5 parts by mass to 6 parts by mass.
[0011] In some embodiments, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.01 parts by mass to 0.08 parts by mass, and / or the trinitrile compound is in an amount of 0.5 parts by mass to 3.5 parts by mass.
[0012] In some embodiments, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.11 parts by mass to 0.85 parts by mass, and / or the trinitrile compound is in an amount of 1.7 parts by mass to 4.6 parts by mass.
[0013] In some embodiments, the electrolyte further includes other additives, and the other additives include at least one of succinonitrile, adiponitrile, ethylene glycol di(propionitrile) ether, lithium monofluorophosphate, 1,2-bis(difluorophosphine oxide)ethane, 1,2-bis(difluorophosphine oxide)propane, 1,2-bis(difluorophosphine oxide)butane, vinylene carbonate, lithium fluorosulfonate, 1,3-propane sultone or vinyl sulfate.
[0014] In some embodiments, the other additives are present in an amount of 0.1 to 6 parts by mass relative to 100 parts by mass of the electrolyte.
[0015] In another aspect of the present application, the present application provides an electronic device, which includes the secondary battery described in the present application.
[0016] The present application uses a specific positive electrode composition and electrolyte combination, which can not only improve the positive electrode's resistance to shedding, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0017] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION
[0018] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.
[0019] Unless expressly stated otherwise, the following terms used in this application have the meanings indicated below.
[0020] The present application uses a specific positive electrode composition and electrolyte combination, which can not only improve the positive electrode's resistance to shedding, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0021] In one embodiment, the present application provides a secondary battery, which includes a positive electrode, a negative electrode, and an electrolyte as described below.
[0022] I. Positive electrode
[0023] The present application relates to a secondary battery and an electronic device. Specifically, the present application provides a secondary battery, which includes: a positive electrode, a negative electrode and an electrolyte, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material and polyvinyl butyral, and the electrolyte includes lithium difluorophosphate and a trinitrile compound, which can not only improve the positive electrode's resistance to shedding, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0024] The positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on a surface of the positive electrode current collector.
[0025] The positive electrode active material layer contains a positive electrode active material, and the positive electrode active material layer may be one layer or multiple layers. The positive electrode active material is any material that can reversibly insert and release lithium ions.
[0026] The inventors of the present application unexpectedly discovered in experiments that, in the process of mixing the positive electrode slurry, the stability of the slurry is improved by adding polyvinyl butyral, but the adhesion of the electrode sheet is reduced. The inventors further discovered that the electrode sheet can significantly improve the adhesion of the electrode sheet in an electrolyte system containing lithium difluorophosphate and trinitrile compounds. It is speculated that the reason may be that polyvinyl butyral is prone to swelling in the carbonate electrolyte system, while lithium difluorophosphate and trinitrile compounds significantly inhibit the swelling, thereby enhancing the cohesion of the positive electrode active material layer and the adhesion to the current collector, which can not only improve the positive electrode's resistance to shedding, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0027] Specifically, from the viewpoint of improving the positive electrode resistance to falling off, polyvinyl butyral has a particle shape, and the average particle size of polyvinyl butyral is preferably less than 100 μm, more preferably less than 80 μm, further preferably less than 60 μm, particularly preferably less than 40 μm, preferably more than 20 μm, and more preferably more than 30 μm. When the average particle size of polyvinyl butyral is within the above range, it can effectively improve the positive electrode resistance to falling off. And then, the cohesion of the positive active material layer and the improvement of the bonding force with the current collector can usually be achieved.
[0028] Specifically, from the viewpoint of improving the resistance to falling off of the positive electrode, the acetalization degree of polyvinyl butyral is 30mol% to 60mol%, and the acetalization degree of polyvinyl butyral is preferably less than 60mol%, more preferably less than 55mol%, further preferably less than 50mol%, particularly preferably less than 45mol%, preferably more than 30mol%, and more preferably more than 35mol%. When the acetalization degree of polyvinyl butyral is within the above range, it is effective to improve the resistance to falling off of the positive electrode. Furthermore, the cohesion of the positive active material layer and the improvement of the bonding force with the current collector can usually be achieved.
[0029] Specifically, from the viewpoint of improving the positive electrode's resistance to shedding, the average molecular weight of polyvinyl butyral is 3×10 4 Up to 20×10 4 The average molecular weight of polyvinyl butyral is preferably 20×10 4 Below, preferably 15×10 4 Below, further preferably 10×10 4 Below, particularly preferably 8×10 4 Below, preferably 3×10 4 More than 5×10 4 When the average molecular weight of polyvinyl butyral is within the above range, the positive electrode resistance to shedding can be effectively improved. Furthermore, the cohesive force of the positive electrode active material layer and the binding force with the current collector can usually be improved.
[0030] Specifically, from the viewpoint of improving the resistance to falling off of the positive electrode, relative to 100 parts by mass of positive electrode materials (including positive electrode active materials, conductive agents, binders, optional auxiliary agents), the mass of the polyvinyl butyral is 0.3 parts by mass to 3 parts by mass. The mass of polyvinyl butyral is preferably less than 3 parts by mass, more preferably less than 2.5 parts by mass, further preferably less than 2 parts by mass, particularly preferably less than 1.5 parts by mass, preferably more than 0.3 parts by mass, and more preferably more than 0.5 parts by mass. When the mass of polyvinyl butyral is within the above range, the resistance to falling off of the positive electrode can be effectively improved. Furthermore, the cohesion of the positive active material layer and the improvement of the bonding force with the current collector can usually be achieved.
[0031] Specifically, from the viewpoint of reducing the initial resistance of the secondary battery, the positive electrode active material layer further includes an auxiliary agent, and the auxiliary agent includes at least one of propylene glycol laurate, pentaerythritol oleate, polyethylene glycol oleate, polypropylene glycol oleate, polyoxyethylene glycerol, or polyoxypropylene glycerol. The auxiliary agent can inhibit the excessive impedance of the trinitrile compound from forming a coating film on the surface of the positive electrode.
[0032] The positive electrode active material is any material that can reversibly intercalate and deintercalate lithium ions. For example, as the positive electrode active material for a secondary battery, a composite metal oxide containing one or more selected from the group consisting of cobalt, manganese, and nickel and lithium, or a lithium-containing olivine-type phosphate containing one or more selected from iron, cobalt, nickel, and manganese is used. These positive electrode active materials can be used alone or in combination of two or more.
[0033] As such a lithium composite metal oxide, for example, those selected from LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2 (0.01 < x < 1), LiNi x Mn y Co z O2 (x + y + z = 1), a solid solution of Li2MnO3 and LiMO2 (M is a transition metal such as Co, Ni, Mn, Fe, etc.), LiNi 1 / 2 Mn 3 / 2 O4, LiFePO4, LiMnPO4, and LiMn 1-x Fe x PO4 (0.01 < x < 1), and more preferably two or more. A part of these composite metal oxides with lithium or lithium-containing olivine-type phosphates can be substituted with other elements, or a part of cobalt, nickel, manganese, and iron can be substituted with one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or coated with a compound or carbon material containing these other elements.
[0034] As the voltage during charging, from the viewpoint of increasing the voltage, the positive electrode potential is preferably 4.4 V (vs. Li / Li + ) or more, more preferably 4.5 V (vs. Li / Li + ) or more, and particularly preferably 4.6 V (vs. Li / Li + ) or more.
[0035] There is no limitation on the type of positive electrode conductive material, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black; carbon materials such as amorphous carbon such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.
[0036] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, and the positive electrode binder. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media consisting of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran; amides such as N-methylpyrrolidone, dimethylformamide, and dimethylacetamide; non-protonic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.
[0037] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.
[0038] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode active material layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.
[0039] The positive electrode can be made by forming a positive electrode active material layer containing a positive electrode active material and a binder on the positive electrode current collector. The manufacture of the positive electrode using the positive electrode active material can be carried out by conventional methods, that is, the positive electrode active material and the binder, as well as the conductive material and the thickener as required, are dry-mixed to form a sheet, and the obtained sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and the slurry is applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode.
[0040] II. Electrolyte
[0041] The electrolyte used in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte. In some embodiments, the electrolyte of the present application includes lithium difluorophosphate and a trinitrile compound.
[0042] Since polyvinyl butyral is prone to swelling in carbonate electrolyte systems, the inventors have found that when the electrolyte contains lithium difluorophosphate and trinitrile compounds, the swelling can be significantly inhibited, thereby increasing the cohesion of the positive electrode active material layer and the adhesion to the current collector, which can not only improve the positive electrode's resistance to detachment, but also reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0043] Specifically, from the perspective of improving the low temperature rate characteristics of the secondary battery, in some embodiments, relative to 100 parts by mass of the electrolyte, the mass of lithium difluorophosphate is a parts by mass, and the value range of a is 0.01 to 1.5. In some embodiments, the value range of a is 0.01 to 0.08. In some embodiments, the value range of a is 0.11 to 0.85. In some embodiments, a is 0.01, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.11, 0.13, 0.35, 0.52, 0.67, 0.85, 1.1, 1.5 or in the range consisting of any two of the above values. For example, 0.01 to 0.05, 0.03 to 0.08, 0.05 to 0.09, 0.03 to 0.13, 0.08 to 0.35, 0.09 to 0.52, 0.13 to 0.67, 0.35 to 0.85, 0.52 to 1.1. When within the above range, it helps to further improve the low temperature rate characteristics.
[0044] Specifically, the trinitrile compound is selected from at least one of 1,2,3-propanetricarbonitrile, 1,3,5-pentanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,4-tris(2-cyanoethoxy)butane, 1,2,3-tris(2-cyanoethoxy)propane, 1,1,1-tris(cyanoethoxymethylene)ethane, 1,1,1-tris(cyanoethoxymethylene)propane, 3-methyl-1,3,5-tris(cyanoethoxy)pentane, 1,2,7-tris(cyanoethoxy)heptane, 1,2,6-tris(cyanoethoxy)hexane, or 1,2,5-tris(cyanoethoxy)pentane. The trinitrile compound may be only one or more.
[0045] Specifically, from the viewpoint of reducing the initial resistance of the secondary battery, in some embodiments, relative to 100 parts by mass of the electrolyte, the mass of the trinitrile compound is b parts by mass, and the value range of b is 0.5 to 6. In some embodiments, the value range of b is 0.5 to 3.5. In some embodiments, the value range of b is 1.7 to 4.6. In some embodiments, b is 0.5, 0.8, 1.3, 1.7, 2.6, 3.4, 4.6, 5.1, 5.5, 6 or in the range consisting of any two of the above values. For example, 0.5 to 3.5, 0.8 to 2.6, 1.3 to 4.6, 1.7 to 3.4, when within the above range, it helps to further improve the low temperature rate characteristics. If it is 2 or more trinitrile compounds, b is the total content.
[0046] In addition, the electrolyte may also include other additives. The inventors also unexpectedly discovered that other additives can not only inhibit the decomposition of polyvinyl butyral during the charging and discharging process, but also further reduce the impedance of the trinitrile coating, thereby further improving the positive electrode's resistance to shedding, reducing the initial resistance of the secondary battery and improving the low-temperature rate characteristics.
[0047] Other additives include at least one of succinonitrile, adiponitrile, ethylene glycol di(propionitrile) ether, lithium monofluorophosphate, 1,2-bis(difluorophosphine oxide)ethane, 1,2-bis(difluorophosphine oxide)propane, 1,2-bis(difluorophosphine oxide)butane, vinylene carbonate, lithium fluorosulfonate, 1,3-propane sultone or vinyl sulfate. The other additives may be only one or more.
[0048] The content of other additives is 0.1 parts by mass or more, preferably 0.3 parts by mass or more, preferably 1.6 parts by mass or more, and more preferably 2.8 parts by mass or more, relative to 100 parts by mass of the electrolyte.
[0049] Furthermore, from the viewpoint of improving low-temperature rate characteristics, the content of other additives is 6 parts by mass or less, preferably 5.7 parts by mass or less, more preferably 4.2 parts by mass or less, and further preferably 3.1 parts by mass or less.
[0050] In some embodiments, the total content of other additives is c parts by mass, and c is 0.1, 0.3, 0.35, 0.4, 0.45, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 1.6, 2, 2.5, 2.9, 3, 3.5, 3.9, 4, 4.5, 5, 5.7, 6 or in the range consisting of any two of the above values. For example, 0.3 to 5.2, 0.45 to 4.5, 0.6 to 3.7, 0.45 to 3.9, 0.7 to 4.5, when within the above range, it helps to further improve the low temperature rate characteristics. If there are more than two other additives, c is the total content.
[0051] The lithium salt used in the electrolyte of the present application includes lithium hexafluorophosphate, and the content of lithium hexafluorophosphate is 9% to 15% by mass, preferably 9% to 13% by mass, and more preferably 9% to 12% by mass, based on the total mass of the electrolyte. By setting the content range to the above, the resistance characteristics and low temperature characteristics can be improved in a more balanced manner.
[0052] The electrolyte of the present application may further include any non-aqueous solvent known in the prior art that can be used as a solvent for the electrolyte. For example, cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, cyclic ethers, chain ethers, phosphorus-containing organic solvents, and sulfur-containing organic solvents. Chain carboxylates are preferred, such as ethyl acetate, ethyl fluoroacetate, ethyl propionate, and propyl propionate.
[0053] In some embodiments, the electrolyte is not particularly limited, and any substance known as an electrolyte can be used arbitrarily. The quality of the electrolyte is not particularly limited as long as it does not impair the effects of the present application.
[0054] III. Negative electrode
[0055] The negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, wherein the negative electrode active material layer contains a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.
[0056] As a current collector for holding the negative electrode active material, any known current collector can be used. Examples of negative electrode current collectors include, but are not limited to, metal materials such as copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper.
[0057] There is no particular limitation on the negative electrode active material, as long as it can reversibly absorb and release lithium ions. Examples of negative electrode active materials may include, but are not limited to, carbon materials such as natural graphite and artificial graphite; metals such as silicon (Si) and tin (Sn); or oxides of metal elements such as Si and Sn. Negative electrode active materials may be used alone or in combination.
[0058] The negative electrode active material layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the negative electrode current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.
[0059] The negative electrode can be prepared by applying a negative electrode mixture slurry containing a negative electrode active material, a resin binder, etc. on a negative electrode current collector, drying it, and then rolling it to form a negative electrode active material layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.
[0060] IV. Isolation membrane
[0061] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.
[0062] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polyether sulfones, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.
[0063] The isolation film may also be a material formed by laminating the above materials, and examples thereof include, but are not limited to, a three-layer isolation film formed by laminating polypropylene, polyethylene, and polypropylene in this order.
[0064] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.) The form of the inorganic material may include, but is not limited to, granular or fibrous.
[0065] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators may also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a resin as an adhesive to form a porous layer on both sides of the positive electrode with aluminum oxide particles having a particle size of 90% less than 1 μm.
[0066] The thickness of the isolation film is arbitrary. In some embodiments, the thickness of the isolation film is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the isolation film is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the isolation film is within the above range, the insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.
[0067] The present application further provides an electronic device, which includes the secondary battery described in the present application.
[0068] The use of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.
[0069] The preparation of the secondary battery is described below in conjunction with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.
[0070] Preparation of secondary batteries
[0071] The positive electrode active material lithium cobalt oxide (97 parts by mass) and acetylene black (1.5 parts by mass) are mixed, added to the solution obtained by dissolving polyvinyl butyral (1.5 parts by mass) shown in Table 1-1 in 1-methyl-2-pyrrolidone, and mixed to prepare a positive electrode mixture paste. The positive electrode mixture paste is applied to an aluminum foil, dried, pressurized, and cut into a specified size to make a positive electrode. If an auxiliary agent (as shown in Table 1-2) is added, the content of polyvinyl butyral is adjusted to 1.3 parts by mass and the auxiliary agent is 0.2 parts by mass.
[0072] The negative electrode active material artificial graphite and silicon carbon (mass ratio 97:3, totaling 96 parts by mass) and styrene-butadiene rubber (2 parts by mass) were mixed and added to a solution obtained by dissolving lithium carboxymethyl cellulose (2 parts by mass) in deionized water in advance and mixed to prepare a negative electrode mixture paste. The negative electrode mixture paste was applied to a copper foil, dried, pressurized, and then cut into a specified size to make a negative electrode.
[0073] A 5 μm polyethylene porous film was used as a separator.
[0074] The positive electrode and negative electrode prepared as above are each connected to a wire. The layers are stacked and wound via the above-mentioned separator. In addition, LiPF6 as a supporting electrolyte is dissolved in a solution containing ethylene carbonate, propylene carbonate, propyl propionate, ethyl propionate, lithium difluorophosphate, trinitrile compounds, and other additives. Based on 100 parts by mass of the total mass of the electrolyte, the mass content and components of lithium difluorophosphate, trinitrile compounds, and other additives are shown in Tables 1-3 and Tables 2, 3, and 4. The mass content of LiPF6 is 14%, and the rest is ethylene carbonate, propylene carbonate, propyl propionate, and ethyl propionate (mass ratio 0.8:1:2:1).
[0075] Then, the wound body and 3.2g of electrolyte were placed in an aluminum laminate case. The opening of the case was heat-sealed, and a secondary battery was made through steps such as formation and capacity measurement. The secondary battery was a pouch-shaped secondary battery with a width of 35mm, a height of 48mm, and a thickness of 5mm.
[0076] Table 1 Table 1-1 Polyvinyl butyral (abbreviated as PVB)
[0077] serial number feature PVB-1 <![CDATA[Particulate, average particle size of 40 microns, degree of acetalization of 46 mol%, average molecular weight of 5×10 4 > PVB-2 <![CDATA[Particulate, with an average particle size of 60 microns, an acetalization degree of 40 mol%, and an average molecular weight of 6.2×10 4 > PVB-3 <![CDATA[Particulate, with an average particle size of 80 microns, an acetalization degree of 55 mol%, and an average molecular weight of 7.9×10 4 >
[0078] Table 1-2 Additives
[0079] serial number name Additive 1 Propylene glycol laurate Additive 2 Pentaerythritol oleate Additive 3 Polyethylene glycol oleate Additive 4 Polyoxypropylene glycerin Additive 5 Polypropylene glycol oleate Additive 6 Polyoxyethylene glycerol
[0080] Table 1-3 Abbreviations of electrolyte components
[0081] Code name Code name N1 1,3,6-hexanetricarbonitrile C1 Succinonitrile N2 1,3,5-Pentatricarboxynitrile C2 Adiponitrile N3 1,2,6-hexanetricarbonitrile C3 Ethylene glycol di(propionitrile) ether N4 1,2,3-Tris(2-cyanoethoxy)propane C4 1,2-Bis(difluorophosphine)ethane N5 1,2,4-Tris(2-cyanoethoxy)butane C5 1,2-Bis(difluorophosphino)propane N6 1,2,5-Tris(cyanoethoxy)pentane C6 1,2-Bis(difluorophosphine)butane C7 Vinylene carbonate C9 1,3-Propane sultone C8 Lithium Fluorosulfate C10 Vinyl Sulfate
[0082] Test Method
[0083] Positive electrode resistance to shedding
[0084] After the prepared secondary battery is injected with electrolyte, it is left to stand at a temperature of 25°C for 6 hours. Next, the battery cell voltage is charged to 4.6V by a constant current method at a temperature of 25°C and 0.1C, and then an aging treatment is performed at a temperature of 60°C for 12 hours. After that, the battery cell is disassembled and the positive electrode is taken out in a state of charging to 4.6V at 0.2C and discharging to 3.0V at 0.2C. The removed positive electrode is washed with diethyl carbonate, the surface of the positive electrode is visually observed, and evaluated according to the following criteria. The fewer cracks and peeling on the surface of the positive electrode, the more it can suppress the positive electrode active material from falling off from the current collector, and the better the resistance to falling off.
[0085] A: Cracks and peeling were observed in an area of 0% or more and less than 3% of the entire positive electrode surface.
[0086] B: Cracks and peeling are observed in an area of 3% or more and less than 5% of the entire positive electrode surface.
[0087] C: Cracks and peeling are observed in an area of 5% or more and less than 10% of the entire positive electrode surface.
[0088] D: Cracks and peeling are observed in 10% or more of the entire positive electrode surface area.
[0089] Initial resistance characteristics of secondary batteries
[0090] The secondary battery was charged at a constant current of 0.2C until the battery voltage reached 4.6V, and then charged at a constant voltage of 4.6V until the charging current reached 0.02C. Next, the battery was discharged at a constant current of 0.2C until the battery voltage reached 3.87V (state of charge (SOC) 50%), and then the voltage change after 30 seconds of discharge at 0.2C, 0.5C, 1.0C, 2.0C, 2.5C, and 3.0C was measured. Each discharge current and the measured voltage change are plotted (horizontal axis: discharge current value, vertical axis: voltage change value), and the slope is used as the resistance value (Ω). The calculated resistance value is evaluated using the following benchmark. The lower the resistance value, the smaller the internal resistance of the secondary battery and the lower the battery resistance.
[0091] A: The resistance value is less than 4Ω.
[0092] B: The resistance value is 4Ω or more and less than 5Ω.
[0093] C: The resistance value is 5Ω or more and less than 6Ω.
[0094] D: The resistance value is 6Ω or more.
[0095] Low temperature rate characteristics of secondary batteries
[0096] After the secondary battery was left standing at 25°C for 24 hours, it was charged at a constant current of 0.1C for 5 hours at 25°C, and the voltage V0 after charging was measured. Then, it was discharged at a discharge rate of 0.5C at -30°C, and the voltage V1 was measured 15 seconds after the start of discharge. Furthermore, the voltage change ΔV represented by ΔV=V0-V1 was obtained and judged according to the following criteria. The smaller the value of the voltage change ΔV, the better the low-temperature rate characteristics.
[0097] A: The voltage change ΔV is less than 0.3V.
[0098] B: The voltage change ΔV is greater than or equal to 0.3V and less than 0.5V.
[0099] C: The voltage change ΔV is greater than or equal to 0.5V and less than 0.8V.
[0100] D: The voltage change ΔV is greater than or equal to 0.8V and less than 1.0V.
[0101] E: The voltage change ΔV is 1.0V or more.
[0102] Test Results
[0103] Table 2
[0104] Binder a Trinitrile compound (b) Fall-off resistance Initial resistance Low temperature rate Example 1-1 PVB-1 0.01 N1(0.5) B B B Example 1-2 PVB-2 0.03 N2(6) B B B Examples 1-3 PVB-3 0.05 N1(1.2) B B B Examples 1-4 PVB-3 0.06 N4(1.2) A B B Examples 1-5 PVB-2 0.07 N5(1.2) A B B Examples 1-6 PVB-2 0.08 N6(1.2) A B B Examples 1-7 PVB-2 0.09 N1(1.2)+N2(0.8) A B B Examples 1-8 PVB-2 0.11 N1(1.2)+N3(0.5) A B B Examples 1-9 PVB-2 0.13 N1(1.2)+N4(0.8) A A B Examples 1-10 PVB-2 0.35 N2(1.2)+N4(0.8) A A B Embodiment 1-11 PVB-2 0.52 N2(1.2)+N5(0.8) A A B Examples 1-12 PVB-2 0.67 N1(1.2)+N4(1.4) A A B Examples 1-13 PVB-2 0.85 N1(1.2)+N4(2.3) A A B Examples 1-14 PVB-2 1.1 N1(2.1)+N4(2.5) A A B Examples 1-15 PVB-2 1.5 N3(1.7) A B B Comparative Example 1-1 PVB-2 0 0 D D E Comparative Example 1-2 PVB-2 0.03 0 D D E Comparative Examples 1-3 PVB-2 0 N1(1.2) D D E Comparative Examples 1-4 PVDF 0 N1(1.2) D D E
[0105] Table 3
[0106]
[0107] Table 4
[0108]
[0109]
[0110] In Tables 2 to 4, relative to 100 parts by mass of the electrolyte, a is the mass fraction of lithium difluorophosphate, b is the mass fraction of the trinitrile compound, and the numbers in () represent the mass fractions of the corresponding substances.
[0111] When the positive electrode active material layer includes a positive electrode active material and polyvinyl butyral, and the electrolyte includes lithium difluorophosphate and a trinitrile compound, not only can the positive electrode's resistance to shedding be improved, but also the initial resistance of the secondary battery can be reduced and the low-temperature rate characteristics can be improved. In particular, when the electrolyte includes at least two of the above trinitrile compounds, the initial resistance of the secondary battery can be further reduced by combining with lithium difluorophosphate.
[0112] In particular, when the positive electrode active material layer also includes auxiliary agents, such as propylene glycol laurate, pentaerythritol oleate, polyethylene glycol oleate, and polyoxypropylene glycerol, it can suppress the excessive impedance of the trinitrile compound forming a film on the positive electrode surface, further reduce the initial resistance of the secondary battery and improve the low-temperature rate characteristics.
[0113] In particular, when the electrolyte also contains other additives, the inventors unexpectedly discovered that the other additives not only inhibit the decomposition of polyvinyl butyral during the charge and discharge process, but also further reduce the impedance of the trinitrile film, thereby further improving the positive electrode's resistance to shedding, reducing the initial resistance of the secondary battery and improving the low-temperature rate characteristics. In particular, when the electrolyte includes at least two of the above-mentioned other additives, the initial resistance and low-temperature rate of the secondary battery are further improved.
[0114] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics in the present application may be combined in one or more embodiments or examples in any suitable manner.
[0115] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.
Claims
1. A secondary battery, characterized in that: It includes: A positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material and polyvinyl butyral, and the electrolyte comprises lithium difluorophosphate and a trinitrile compound.
2. The secondary battery according to claim 1, characterized in that: The polyvinyl butyral has at least one of the following characteristics: Feature 1. It has a particle shape and an average particle size of 20 microns to 100 microns; Feature 2: The degree of acetalization is 30 mol% to 60 mol%; Feature 3: Average molecular weight is 3×10 4 Up to 20×10 4 .
3. The secondary battery according to claim 1 or 2, characterized in that: The positive electrode active material layer further comprises an auxiliary agent, and the auxiliary agent comprises at least one of propylene glycol laurate, pentaerythritol oleate, polyethylene glycol oleate, polypropylene glycol oleate, polyoxyethylene glyceryl ether or polyoxypropylene glyceryl ether.
4. The secondary battery according to claim 1 or 2, characterized in that: The trinitrile compound is selected from at least one of 1,2,3-propanetricarboxylate, 1,3,5-pentanetricarboxylate, 1,2,6-hexanetricarboxylate, 1,3,6-hexanetricarboxylate, 1,2,4-tris(2-cyanoethoxy)butane, 1,2,3-tris(2-cyanoethoxy)propane, 1,1,1-tris(cyanoethoxymethylene)ethane, 1,1,1-tris(cyanoethoxymethylene)propane, 3-methyl-1,3,5-tris(cyanoethoxy)pentane, 1,2,7-tris(cyanoethoxy)heptane, 1,2,6-tris(cyanoethoxy)hexane or 1,2,5-tris(cyanoethoxy)pentane.
5. The secondary battery according to claim 1, characterized in that: Wherein, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.01 parts by mass to 1.5 parts by mass, and / or the trinitrile compound is in an amount of 0.5 parts by mass to 6 parts by mass.
6. The secondary battery according to claim 1, characterized in that: Wherein, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.01 parts by mass to 0.08 parts by mass, and / or the trinitrile compound is in an amount of 0.5 parts by mass to 3.5 parts by mass.
7. The secondary battery according to claim 1, characterized in that: Wherein, relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is in an amount of 0.11 parts by mass to 0.85 parts by mass, and / or the trinitrile compound is in an amount of 1.7 parts by mass to 4.6 parts by mass.
8. The secondary battery according to any one of claims 1, 2, 5 to 7, characterized in that: The electrolyte further includes other additives, and the other additives include at least one of succinonitrile, adiponitrile, ethylene glycol di(propionitrile) ether, monofluorolithium phosphate, 1,2-bis(difluorophosphine oxide)ethane, 1,2-bis(difluorophosphine oxide)propane, 1,2-bis(difluorophosphine oxide)butane, vinylene carbonate, lithium fluorosulfonate, 1,3-propane sultone or vinyl sulfate.
9. The secondary battery according to claim 8, characterized in that: The other additives are present in an amount of 0.1 to 6 parts by mass relative to 100 parts by mass of the electrolyte.
10. An electronic device, characterized in that: It includes the secondary battery according to any one of claims 1 to 9.
Citation Information
Cited By
Negative pole piece, electrochemical device and preparation method of negative pole piece
CN120511303A
Electrolyte, secondary battery and electronic device
WO2026184327A1