Battery pack bottom protection plate, battery pack comprising same and vehicle
By using a coating with high Young's modulus and appropriate stress on the bottom protective plate of the battery pack, the problems of coating wear and friction and slippage during the transmission of the power battery pack in the battery swap station are solved, extending the service life of the battery pack and improving the efficiency of the battery pack. Battery exchange efficiency.
Patent Information
- Application Number
- CN202411120202.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-22
AI Technical Summary
During the transmission of power battery packs on chains or rollers in power swap stations, the coating of the bottom guard plate is prone to wear and tear, resulting in shortened service life, and dynamic and static friction and slippage are prone to occur, affecting the battery swap efficiency and the service life of the battery pack.
Use a coating with Young's modulus ≥5MPa, the maximum stress before tensile fracture is 2MPa-50MPa, and the maximum strain is 2%-100% to improve the wear resistance and anti-friction ability of the coating to ensure circulation in the power swap station After 1500 times, the bottom guard plate will not wear out and avoid slipping due to dynamic and static friction.
It extends the service life of the battery pack, improves the efficiency of the battery swap station, ensures that the coating will not wear out under high-frequency friction, and can withstand the pressure of the battery pack without cracking or damage.
Smart Images

Figure BDA0004995203080000101 
Figure BDA0004995203080000102 
Figure BDA0004995203080000103
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a battery pack bottom guard plate and a battery pack and a vehicle containing the same. Background Art
[0002] In the past two years, the domestic new energy vehicle market has shown a rapid growth trend. With the rapid development of new energy, how to build a complete energy replenishment system has become an unavoidable problem. At present, there are two ways to replenish pure electric energy in China. One is the more common construction of charging piles, and the other is to deploy battery swap stations like NIO. On the one hand, the battery swap system has an overwhelming advantage in energy replenishment efficiency. For example, it is more convenient and faster for users. On the other hand, since the battery swap station manages the battery in a unified manner, all users no longer need to worry about battery degradation and safety issues, and they can get a battery check every time they swap the battery.
[0003] At present, the warranty period of power batteries is generally 8 years. Battery companies do not have much economic motivation to extend the service life of batteries after selling batteries or vehicle manufacturers that adopt the charging and energy replenishment route after selling vehicles. For NIO, which adopts the battery replacement and energy replenishment route, if the service life of the battery can be extended, it can bring huge economic benefits. At present, NIO plans to promote 15 years of worry-free battery service and increase the warranty period of power batteries from 8 years to 15 years, which puts more stringent requirements on the service life of existing batteries. However, there are few existing technical reports on how to increase the service life of power batteries to 15 years. Summary of the invention
[0004] The applicant has discovered that when a battery pack is replaced and recharged, it needs to be transported and circulated at the battery swap station via chains or rollers. During the transmission process, the bottom protective plate of the battery pack will inevitably come into contact with the chains or rollers, generating friction. If the wear resistance of the coating on the bottom protective plate of the battery pack is poor, the coating will become thinner or even expose the metal bottom plate, increasing the risk of the metal bottom plate being exposed or even corroded or punctured by external forces, thus affecting the service life of the battery pack.
[0005] At present, the coating of the bottom guard plate of the battery pack is often made of solvent-based polyvinyl chloride (PVC) coating to achieve the effect of corrosion resistance and stone impact resistance, but the wear resistance of the coating is not considered. Taking the second-generation battery swap station of NIO as an example, the transmission parts used for battery swap transmission in the battery swap station include chains and rollers. When the battery pack is in circulation, the bottom guard plate of the battery pack will have sliding friction with the nitrile rubber chain cover and the polyurethane roller, and there will also be static friction with the nitrile rubber chain cover. The existing battery pack with PVC coated bottom guard plate will be worn after 500-800 power swaps at the battery swap station, exposing the anti-corrosion layer underneath, thus affecting the service life of the battery pack. If the service life of the battery pack is to be increased to 15 years, according to the normal frequency of use, the battery pack ideally needs to be able to circulate in the battery swap station 1500 times without wearing out the bottom guard plate coating and not have dynamic and static friction and slipping when circulating in the battery swap station.
[0006] The first aspect of the present application provides a battery pack bottom guard plate, comprising a metal plate and a coating arranged on the surface of the metal plate, the Young's modulus of the coating being ≥5MPa, the maximum stress of the coating before tensile fracture being 2MPa-50MPa, and the maximum strain of the coating before tensile fracture being 2%-100%.
[0007] A second aspect of the present application provides a battery pack, which includes the battery pack bottom guard plate as described in the first aspect, and the coating is arranged on the outer surface of the battery pack.
[0008] A third aspect of the present application provides a vehicle, comprising the battery pack as described in the second aspect, wherein the battery pack is mounted on the bottom of the vehicle.
[0009] The beneficial effects of this application are: this application solves the problem that the bottom guard plate coating of the battery pack is easily worn due to periodic continuous scraping and friction when the battery pack is circulated in the battery swap station, and the problem that the battery pack is prone to dynamic and static friction and slipping when it is circulated in the battery swap station, thereby improving the circulation efficiency of the battery swap station and the service life of the battery pack. In addition, the compressive pressure of the bottom guard plate coating can reach 10g / mm 2 -20g / mm 2 , and can withstand the pressure of the entire battery pack during battery replacement without any cracking, breakage, or peeling of the coating. DETAILED DESCRIPTION
[0010] For simplicity, this application only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.
[0011] In this application, unless otherwise clearly specified and limited, the terms "installed", "set", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, an indirect connection through an intermediate medium, or a connection between the two elements. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0012] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0013] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.
[0014] 1. Battery pack bottom guard plate
[0015] The first aspect of the present application provides a battery pack bottom guard plate, comprising a metal plate and a coating disposed on the surface of the metal plate, wherein the Young's modulus of the coating is ≥5MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-100%. The inventors of the present application have found that by controlling the Young's modulus, maximum stress and maximum strain of the bottom guard plate coating, the wear resistance of the coating can be improved, the number of circulation times of the battery pack can be increased, and the problem of dynamic and static friction slipping during the circulation of the battery pack in the battery pack station can be improved.
[0016] In this application, "maximum stress" refers to the maximum stress value generated inside the coating when the coating is subjected to external force. When the internal stress of the coating exceeds its tolerance limit, the coating will be damaged, cracked, damaged, etc. In this application, "maximum stress" can be measured by conventional testing methods in this field, for example, with reference to the method of GB / T 528; it can also be measured by a tensile testing machine at room temperature (23±2°C) according to a certain tensile rate such as 50mm / min and a certain gauge length such as 25mm.
[0017] In this application, "maximum strain" refers to the maximum strain value that the coating can withstand when subjected to external force, which reflects the rupture point or deformation limit of the coating. In this application, "maximum strain" can be measured by conventional testing methods in the field, such as referring to the method of GB / T 528; it can also be measured by a tensile testing machine at room temperature (23±2℃) according to a certain tensile rate such as 50mm / min and a certain gauge length such as 25mm.
[0018] In this application, "Young's modulus" is also called elastic modulus, which refers to the elasticity range in which an elastic material will produce positive strain when subjected to positive stress. When the deformation does not exceed a certain elastic limit of the corresponding material, the ratio of positive stress to positive strain is defined as the Young's modulus of this material. In this application, "Young's modulus" can be measured by conventional testing methods in the field, for example, with reference to the method of GB / T 528; or a tensile testing machine can be used at room temperature (23±2°C) to obtain a stress-strain curve of the coating at a certain stretching rate such as 50mm / min and a certain gauge length such as 25mm, and then the slope of the curve in the strain range of 0%-5% is calculated to obtain the Young's modulus of the coating.
[0019] In this application, "wear resistance" refers to the ability of the coating surface to resist wear and tear, which is a kind of material durability. "Wear resistance" means that the coating is not easily worn under high-frequency friction, and the surface will not show phenomena such as thinning and peeling of the skin.
[0020] In this application, "battery swap station circulation times" refers to the number of times a battery pack completes a round trip between the battery compartment and the battery swap platform through the battery transfer and conveying system in the battery swap station. Here, the "battery transfer and conveying system" is used to transfer batteries between the battery swap station platform and the battery compartment, the "battery swap platform" is used to locate and swap batteries for the vehicle, and the "battery compartment" is used to store and charge the battery. Taking the second-generation NIO battery swap station as an example, a battery swap station circulation time refers to a battery pack going back and forth through the cache position, docking position, lifting position and battery compartment in the battery swap station.
[0021] In this application, "slipping" includes dynamic friction slipping and static friction slipping. Among them, dynamic friction slipping refers to the situation where the friction between the bottom guard plate of the battery pack and the transmission component of the battery swap station cannot completely offset the relative movement trend between the two, causing the battery pack to slip, including the sliding friction slipping of the battery pack at the polyurethane roller and the sliding friction slipping at the nitrile rubber chain cover. Static friction slipping refers to the situation where the friction between the bottom guard plate of the battery pack and the transmission component of the battery swap station cannot completely offset the external force, causing the battery pack to slip, including the static friction slipping of the battery pack from the nitrile rubber chain cover of one compartment to the nitrile rubber chain cover of another compartment.
[0022] In some embodiments, the Young's modulus of the coating is exemplarily ≥5MPa, ≥50MPa, ≥100MPa, ≥150MPa, ≥200MPa, ≥250MPa, ≥300MPa. If the Young's modulus of the coating is too low, the coating will be deformed greatly under the same pressure conditions, resulting in damage to the coating surface, and even the coating is exposed, thereby affecting the wear resistance of the coating. In some embodiments, the Young's modulus of the coating is exemplarily 5MPa, 8MPa, 20MPa, 50MPa, 100MPa, 150MPa, 200MPa, 250MPa, 300MPa, 350MPa, 400MPa, 500MPa, 550MPa, 600MPa, 650MPa, 700MPa, 750MPa, 800MPa or a range consisting of any two of these values. In some embodiments, the Young's modulus of the coating is 5 MPa-800 MPa. In some preferred embodiments, the Young's modulus of the coating is 200 MPa-700 MPa.
[0023] In some embodiments, the maximum stress before the coating is stretched to fracture is exemplarily 2MPa, 5MPa, 8MPa, 10MPa, 12MPa, 15MPa, 18MPa, 20MPa, 22MPa, 25MPa, 28MPa, 30MPa, 32MPa, 35MPa, 38MPa, 40MPa, 42MPa, 45MPa, 48MPa, 50MPa or a range consisting of any two of these values. If the maximum stress before the coating is stretched to fracture is too low, the coating will be insufficient in its ability to withstand pressure, and will be easily worn or peeled off when subjected to external stress, such as compression, tension, shearing, etc. In some preferred embodiments, the maximum stress before the coating is stretched to fracture should be 5MPa-45MPa.
[0024] In some embodiments, the maximum strain before the coating is stretched to break is exemplarily 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100% or a range consisting of any two of these values. If the maximum strain before the coating is stretched to break is too low, the coating will be unable to withstand pressure and will be easily worn or peeled off when subjected to external stress, such as compression, tension, shear and other forms of force. In some preferred embodiments, the maximum strain before the coating is stretched to break is 2%-50%.
[0025] In some embodiments, the toughness of the coating is 0.5 MPa-8 MPa, exemplarily 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa, 6 MPa, 6.5 MPa, 7 MPa, 7.5 MPa, 8 MPa, or a range consisting of any two of these values.
[0026] In this application, "toughness" refers to the ability of a coating to maintain its integrity and stability when subjected to external forces, and reflects the ability of the coating to resist deformation and damage caused by external forces. In this application, "toughness" can be measured by conventional testing methods in the field, such as referring to the method of GB / T 528; or a tensile testing machine can be used at room temperature (23±2°C) to obtain a stress-strain curve of the coating at a certain tensile rate such as 50mm / min and a certain gauge length such as 25mm, and then the area under the stress-strain curve is calculated to obtain the toughness of the coating.
[0027] In some embodiments, the shear modulus of the coating is 2MPa-300MPa, exemplarily 2MPa, 5MPa, 10MPa, 20MPa, 50MPa, 80MPa, 100MPa, 120MPa, 150MPa, 180MPa, 200MPa, 220MPa, 250MPa, 280MPa, 300MPa or the range of any two of these values. In some preferred embodiments, the shear modulus of the coating is 50MPa-250MPa.
[0028] In this application, "shear modulus" refers to the proportional relationship between stress and strain generated by a coating when subjected to shear stress. In this application, "shear modulus" can be measured according to the formula G = E / (2*(1+ν)), where G is the shear modulus, E is the Young's modulus, and ν is the Poisson's ratio, where the Young's modulus E can be measured using the method described above in this application, and ν can be obtained by looking up technical books or reference books in the field according to the selected coating material.
[0029] In some embodiments, the compression modulus of the coating is 5MPa-900MPa, exemplarily 5MPa, 8MPa, 10MPa, 50MPa, 100MPa, 150MPa, 200MPa, 250MPa, 300MPa, 350MPa, 400MPa, 450MPa, 500MPa, 550MPa, 600MPa, 650MPa, 700MPa, 750MPa, 800MPa, 900MPa or the range of any two of these values. In some preferred embodiments, the compression modulus of the coating is 50MPa-850MPa.
[0030] In this application, "compression modulus" refers to the proportional relationship between stress and strain generated by a coating when subjected to compressive stress. In this application, "compression modulus" can be measured according to the formula K = E / (3*(1-2ν)), where K is the compression modulus, E is the Young's modulus, and ν is the Poisson's ratio, where the Young's modulus E can be measured using the method described above in this application, and ν can be obtained by looking up technical books or reference books in the field according to the selected coating material.
[0031] In some embodiments, the coating material of the coating is selected from one or more of polyester, epoxy and polyamide. In some preferred embodiments, the coating is a powder coating, and the powder coating material of the powder coating is selected from one or more of polyester powder coating, epoxy powder coating and polyamide powder coating, so as to facilitate the coating to better resist high-frequency friction without wear. In some embodiments, the coating is a solvent-based coating or a solvent-free coating, and the coating material of the solvent-based coating or the solvent-free coating includes a solvent-based coating or a solvent-free coating selected from polyester, epoxy and polyamide.
[0032] In some embodiments, the thickness of the coating is 50 μm-500 μm, exemplarily 50 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 220 μm, 240 μm, 260 μm, 280 μm, 300 μm, 350 μm, 400 μm, 420 μm, 450 μm, 480 μm, 500 μm or a range consisting of any two of these values. The thickness of the coating within the above range is more conducive to improving the wear resistance of the coating while taking into account slippage. In some preferred embodiments, the coating is a powder coating, and the thickness of the powder coating is 50 μm-400 μm. In some preferred embodiments, the coating is a powder coating, and the thickness of the powder coating is 50 μm-300 μm.
[0033] In some embodiments, the metal plate is a steel plate or an aluminum alloy.
[0034] In some embodiments, the metal plate is a steel plate. Compared with other metal plates, the steel plate has better tensile strength and elongation, can meet the impact resistance requirements, and is beneficial to improving the protection of the battery pack, thereby increasing the service life of the battery.
[0035] In some embodiments, the thickness of the metal plate is 0.7 mm-1.5 mm, exemplarily 0.7 mm, 0.9 mm, 1.1 mm, 1.3 mm, 1.5 mm or a range consisting of any two of these values. In some embodiments, the thickness of the metal plate is 0.8 mm-1 mm.
[0036] In some embodiments, an anti-corrosion layer is further provided between the metal plate and the coating to further improve the anti-corrosion performance of the metal plate. The anti-corrosion layer may be an electrophoretic layer or a primer layer, as long as the electrophoretic layer or the primer layer can effectively isolate the metal plate from the external environment of the battery pack as a protective layer, and protect the metal plate from environmental erosion, especially when the coating is damaged, the metal plate is protected from external environmental erosion, thereby improving the service life of the battery pack.
[0037] In some embodiments, the anti-corrosion layer has a thickness of 20 μm-60 μm, exemplarily 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm or a range consisting of any two of these values.
[0038] In some embodiments, the anticorrosion layer is an epoxy electrophoretic paint layer, an acrylate electrophoretic paint layer, an acrylic electrophoretic paint layer, a polyurethane electrophoretic paint layer, a polyester electrophoretic paint layer, an epoxy primer layer, a polyacrylic primer layer or a polyester primer layer. In some preferred embodiments, the anticorrosion layer is an epoxy primer layer or an epoxy electrophoretic paint layer.
[0039] In some embodiments, the battery pack bottom guard plate includes a metal plate and a coating arranged on the surface of the metal plate, no anti-corrosion layer is arranged between the metal plate and the coating, the Young's modulus of the coating is ≥5MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-100%.
[0040] In some embodiments, the battery pack bottom guard plate includes a metal plate and a coating arranged on the surface of the metal plate, no anti-corrosion layer is arranged between the metal plate and the coating, the Young's modulus of the coating is 5MPa-800MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-50%.
[0041] In some embodiments, the battery pack bottom guard plate includes a metal plate and a coating arranged on the surface of the metal plate, the anti-corrosion layer is also arranged between the metal plate and the coating, the Young's modulus of the coating is ≥5MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-100%.
[0042] In some embodiments, the battery pack bottom guard plate includes a metal plate and a coating arranged on the surface of the metal plate, the anti-corrosion layer is also arranged between the metal plate and the coating, the Young's modulus of the coating is 5MPa-800MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-50%.
[0043] In some embodiments, the thickness of the battery pack bottom guard plate is 0.7 mm-1.5 mm, exemplarily 0.7 mm, 0.9 mm, 1.1 mm, 1.3 mm, 1.5 mm, or a range consisting of any two of these values. In some embodiments, the thickness of the battery pack bottom guard plate is 0.8 mm-1 mm.
[0044] In some embodiments, the compressive pressure of the coating is 10 g / mm 2 -20g / mm 2 , exemplarily 10 g / mm 2 , 12g / mm 2 , 14g / mm 2 , 16g / mm 2 , 18g / mm 2 , 20g / mm 2 Or a range consisting of any two of these values. When the battery pack is replaced, the bottom guard plate needs to withstand the pressure of the entire battery pack, and accordingly the coating on the bottom guard plate also needs to withstand the pressure of the entire battery pack, otherwise it will cause cracking, damage, peeling, etc. of the coating.
[0045] 2. Battery Pack
[0046] The second aspect of the present application provides a battery pack, which includes the battery pack bottom guard plate as described in the first aspect, and the coating is arranged on the outer surface of the battery pack. The coating is arranged on the outer surface of the battery pack to improve the wear resistance of the battery pack and solve the problem that the battery pack is easy to slip when it is circulated in the battery swap station.
[0047] 3. Vehicles
[0048] A third aspect of the present application provides a vehicle, comprising a battery pack as described in the second aspect, wherein the battery pack is installed on the vehicle. In some embodiments, the battery pack is installed on the bottom of the vehicle. When the battery pack is installed, the bottom guard plate of the battery pack is arranged toward the ground.
[0049] In some embodiments, the battery pack is mounted on a chassis of the vehicle, and the battery pack bottom guard plate is disposed away from the chassis.
[0050] In some embodiments, the vehicle is a battery-swappable vehicle. In this application, a battery-swappable vehicle generally refers to all vehicles that support a battery-swappable function. In some embodiments, the vehicle has a structure for replacing the battery pack.
[0051] In some embodiments, the vehicle includes, but is not limited to, an electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.
[0052] Example
[0053] In the present application, the methods in the examples, unless otherwise specified, are all conventional methods in the art; the raw materials, materials, and reagents in the examples, unless otherwise specified, are all commercially available conventional raw materials, materials, or reagents.
[0054] Test Method
[0055] 1. Determination of maximum stress and maximum strain of coating
[0056] The maximum stress and maximum strain before tensile fracture of the bottom guard plate coating of each embodiment and comparative example were measured with reference to the method of GB / T 528. The testing instrument was a tensile testing machine, the gauge length used in the test was 25 mm, the tensile rate was 50 mm / min, the test sample size was in accordance with the dumbbell-shaped type I specimen of GB / T 528, and the sample thickness was input into the tensile testing machine according to the actual measured data of the film thickness meter.
[0057] 2. Determination of Young's modulus, toughness, shear modulus and compression modulus of coating
[0058] The stress-strain curves of the bottom guard plate coatings of the embodiments and comparative examples were measured with reference to the method of GB / T 528. The testing instrument was a tensile testing machine, the gauge length used in the test was 25 mm, the tensile rate was 50 mm / min, the test sample size was in accordance with the dumbbell-shaped type I specimen of GB / T 528, and the sample thickness was input into the tensile testing machine according to the actual measured data of the film thickness meter.
[0059] The Young's modulus of the coating is obtained by calculating the slope of the curve within the strain range of 0%-5% based on the obtained stress-strain curve.
[0060] The toughness of the coating is obtained by calculating the area under the stress-strain curve.
[0061] The shear modulus of the coating is measured according to the formula G=E / (2*(1+ν)), where G is the shear modulus, E is the Young's modulus, and ν is the Poisson's ratio. The Poisson's ratio of Example 1 is 0.37, the Poisson's ratio of Example 2 is 0.35, the Poisson's ratio of Example 3 is 0.32, the Poisson's ratio of Comparative Example 1 is 0.25, and the Poisson's ratio of Comparative Example 2 is 0.32.
[0062] The compression modulus of the coating is measured according to the formula K=E / (3*(1-2ν)), where K is the compression modulus, E is the Young's modulus, and ν is the Poisson's ratio. The Poisson's ratio of Example 1 is 0.37, the Poisson's ratio of Example 2 is 0.35, the Poisson's ratio of Example 3 is 0.32, the Poisson's ratio of Comparative Example 1 is 0.25, and the Poisson's ratio of Comparative Example 2 is 0.32.
[0063] 3. Wear resistance test of battery swap station
[0064] The battery pack bottom guard plates of each embodiment and comparative example were subjected to a battery swap test at room temperature in a battery swap station to observe whether the bottom guard plate coating was worn through after the battery pack was switched 1,500 times. "Wear through" here means that the anti-corrosion layer (when there is an electrophoretic layer or primer layer) or the metal plate (when there is no electrophoretic layer or primer layer) under the coating was exposed. When the battery pack circulates in the battery swap station, the bottom guard plate coating of the battery pack will have periodic and continuous back-and-forth friction with the transmission chain and roller of the battery swap station.
[0065] If the coating on the bottom guard plate is not worn through after the converter is switched for 1500 times, the film thickness at three points of the friction mark is measured with a film thickness meter and recorded, and the average value is taken as the film thickness reduction of the coating. The coating is not worn through and the lower the film thickness reduction, the better the wear resistance of the coating.
[0066] 4. Swap station skidding test
[0067] The battery packs containing the bottom guard plates of each embodiment and comparative example were subjected to a battery swap test at room temperature at a battery swap station, and the slippage of the battery packs during circulation in the battery swap station was recorded. When the battery packs circulate in the battery swap station, the bottom guard plates of the battery packs will have sliding friction with the nitrile rubber chain cover and the polyurethane roller, and there will also be static friction with the nitrile rubber chain cover.
[0068] If the battery pack circulates 1500 times in the battery swap station, and the in-place detector does not detect that the battery pack is not in place or is offset in place, and no abnormal noise or idling of the roller is observed, it is considered that there is no dynamic or static friction slip between the bottom guard plate of the battery pack and the upper cover of the nitrile rubber chain, and there is no dynamic friction slip between the polyurethane roller.
[0069] Example 1
[0070] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a thermoplastic powder coating disposed on the surface of the metal plate, and an anti-corrosion layer is disposed between the powder coating and the metal plate. The metal plate is a steel plate, the powder coating is a polyamide (PA11) powder coating, and the anti-corrosion layer is an epoxy electrophoretic layer. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0071] When preparing the bottom guard plate of the battery pack, first electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and then the back of the bottom guard plate substrate is masked with masking tape, and polyamide powder coating is electrostatically sprayed on the front of the bottom guard plate substrate, and then cured at 200-220℃ for 20-35min. The thickness of the cured coating is 261μm, and then the masking tape is removed to obtain the bottom guard plate of the battery pack. See Table 1 for the specific coating material system and curing conditions.
[0072] Example 2
[0073] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a thermosetting powder coating disposed on the surface of the metal plate, and no anti-corrosion layer is disposed between the powder coating and the metal plate. The metal plate is a steel plate, and the powder coating is an epoxy powder coating. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0074] When preparing the battery pack bottom guard plate, the back of the steel plate is first masked with masking tape, and the epoxy powder coating is electrostatically sprayed on the surface of the steel plate, and then cured at 170-200°C for 10-25 minutes. The thickness of the cured coating is 138μm, and then the masking tape is removed to obtain the battery pack bottom guard plate. The specific coating material system and curing conditions are shown in Table 1.
[0075] Example 3
[0076] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a solvent-based coating disposed on the surface of the metal plate, and no anti-corrosion layer is disposed between the solvent-based coating and the metal plate. The metal plate is a steel plate, and the solvent-based coating is a two-component epoxy solvent-based coating. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0077] When preparing the battery pack bottom guard plate, the back of the steel plate is first masked with a masking tape, and then the A and B components of the two-component epoxy solvent-based coating are mixed. The resulting mixture is sprayed on the steel plate surface by liquid spraying, pneumatic spraying or high-pressure airless spraying, and then cured at 80°C for 30 minutes. The thickness of the cured coating is 460μm. After that, the masking tape is removed to obtain the battery pack bottom guard plate. The specific coating material system and curing conditions are shown in Table 1.
[0078] Comparative Example 1
[0079] The battery pack bottom guard plate of this comparative example includes a metal plate as a bottom plate and a solvent-based coating arranged on the surface of the metal plate, and an anti-corrosion layer is also arranged between the solvent-based coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy electrophoretic layer, and the solvent-based coating is a single-component foamed polyvinyl chloride (PVC) solvent-based coating. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0080] When preparing the bottom guard plate of the battery pack, first electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and then the back of the bottom guard plate substrate is masked with masking tape, and the front of the bottom guard plate substrate is sprayed with foaming PVC solvent-based paint by liquid spraying, pneumatic spraying or high-pressure airless spraying, and then foamed and cured at 140°C for 30 minutes. The thickness of the cured coating is 995μm, and then the masking tape is removed to obtain the bottom guard plate of the battery pack. The specific coating material system and curing conditions are shown in Table 1.
[0081] Comparative Example 2
[0082] The battery pack bottom guard plate of this comparative example includes a metal plate as a bottom plate and a solvent-based coating arranged on the surface of the metal plate, and an anti-corrosion layer is also arranged between the solvent-based coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy electrophoretic layer, and the solvent-based coating is a single-component non-foamed polyvinyl chloride (PVC) solvent-based coating. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0083] When preparing the bottom guard plate of the battery pack, first electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and then the back of the bottom guard plate substrate is masked with masking tape, and the front of the bottom guard plate substrate is sprayed with non-foaming PVC solvent-based paint by liquid spraying, pneumatic spraying or high-pressure airless spraying, and then cured at 140°C for 30 minutes. The thickness of the cured coating is 423μm, and then the masking tape is removed to obtain the bottom guard plate of the battery pack. The specific coating material system and curing conditions are shown in Table 1.
[0084] Table 1
[0085]
[0086] Table 2 records the maximum stress and maximum strain before tensile fracture of the bottom guard plate coating of each embodiment and comparative example, as well as the test results of Young's modulus, shear modulus and compression modulus.
[0087] Table 2
[0088]
[0089] Table 3 records the results of the wear resistance test and slip test of the bottom guard plate coating of each embodiment and comparative example at the battery swap station. It can be seen that the bottom guard plates of embodiments 1-3 of the present invention did not wear out after 1500 circulations at the battery swap station and did not slip during the 1500 circulations. In addition, the powder coating of the bottom guard plates of embodiments 1-3 of the present invention can withstand 10g / mm 2 -20g / mm 2 The compressive pressure will not cause cracking, damage or peeling of the coating.
[0090] Table 3
[0091]
[0092]
[0093] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.
Claims
1. A battery pack bottom guard plate, characterized in that: It comprises a metal plate and a coating arranged on the surface of the metal plate, wherein the Young's modulus of the coating is ≥5MPa, the maximum stress of the coating before tensile fracture is 2MPa-50MPa, and the maximum strain of the coating before tensile fracture is 2%-100%.
2. The battery pack bottom guard plate according to claim 1, characterized in that: The Young's modulus of the coating is 5MPa-800MPa, and / or the maximum strain of the coating before tensile fracture is 2%-50%.
3. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: The toughness of the coating is 0.5Mpa-8MPa.
4. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: The shear modulus of the coating is 2MPa-300MPa.
5. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: The compression modulus of the coating is 5MPa-900MPa.
6. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: The coating material of the coating is selected from one or more of polyester, epoxy and polyamide.
7. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: The coating is a powder coating, and / or the coating has a thickness of 50 μm-400 μm.
8. A battery pack, characterized in that: It includes a battery pack bottom guard plate as described in any one of claims 1 to 7, wherein the coating is arranged on the outer surface of the battery pack.
9. A vehicle, characterized in that: Comprising the battery pack as claimed in claim 8, wherein the battery pack is installed in the vehicle.
10. The vehicle according to claim 9, characterized in that The vehicle has a structure for replacing the battery pack.