Pulse current rapid post-treatment method for improving tensile property of selective laser melting IN718 alloy
The non-thermal effects of pulse current treatment and the Joule heating effect work together to promote the recrystallization and grain refinement of the selective laser melted IN718 alloy, solving the complex and high-cost problems of traditional heat treatment, and significantly improving the mechanical properties and plasticity of the alloy. Provides theoretical guidance on new high-temperature alloy applications.
Patent Information
- Application Number
- CN202411121298.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-25
AI Technical Summary
The high cooling rate and thermal gradient of the IN718 high-temperature alloy manufactured by selective laser melting results in uneven microstructure and uneven distribution of brittle precipitates, which reduces the mechanical properties of the alloy. The traditional heat treatment method is complex and costly, making it difficult to be widely used in the engineering field.
The pulse current rapid post-processing method is used to promote metal recrystallization through the Joule heating effect and non-thermal effect of the pulse current, improve the internal dislocation distribution, refine the grains, and improve the tensile properties of the alloy.
The plasticity and tensile strength of the alloy are significantly improved, the processing time is shortened, the energy consumption is reduced, and the structure and properties of the selective laser melted nickel-based high-temperature alloy are controlled.
Smart Images

Figure CN118832191A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of performance improvement of selective laser melted nickel-based high-temperature alloys, and specifically relates to a pulse current rapid post-processing method for improving tensile properties of selective laser melted IN718 alloys. Background Art
[0002] Inconel718 nickel-based superalloy (IN718), domestic grade GH4169 superalloy, is an aging-hardened nickel-based superalloy with face-centered cubic γ′ phase and body-centered cubic γ″ phase as strengthening phases. It is a precipitation-hardened nickel-chromium-iron alloy first developed by the American International Nickel Company in the late 1950s. It is widely used in aerospace, energy industry, and automotive industry. At present, IN718 superalloy is still one of the largest and most widely used nickel-based superalloys. Inconel718 nickel-based superalloy has high tensile strength, good oxidation resistance, corrosion resistance and creep resistance under high temperature conditions, and is therefore widely used in the aerospace industry.
[0003] Inconel718 has good weldability due to its slow precipitation strengthening kinetics, thus minimizing the possibility of cracking. However, due to reasons such as rapid tool wear and low material removal rate, Inconel718 material is difficult to manufacture by traditional machining methods at room temperature. Selective Laser Melting (SLM) technology can effectively solve the above problems. SLM manufactures parts layer by layer by selectively melting and consolidating metal powders using a high-energy laser beam. Compared with traditional casting and forging, SLM has many advantages, such as near-net shaping of complex and difficult-to-machine parts without molds. The process characteristics of SLM are its extremely fast cooling rate of up to 10 7 K / s, faster solidification rate can significantly refine the grains. However, high cooling rate and thermal gradient cause internal stress in parts, which will also lead to uneven structure of IN718 manufactured by SLM additive manufacturing, uneven distribution of a large number of brittle precipitates, and rapid solidification at high cooling rate will lead to directional growth of grains, thereby reducing the mechanical properties of the alloy. Therefore, IN718 manufactured by SLM is not suitable for direct use in the deposited state. Previous studies have mostly solved the above problems through solid solution plus two-stage aging. However, traditional heat treatment methods have complex steps and high costs, and may lead to decreased corrosion resistance and coarse grains, which are unfavorable to mechanical properties, seriously hindering its widespread application in the engineering field. It is urgent to find a new post-processing method. Summary of the invention
[0004] The purpose of the present invention is to provide a pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy, aiming to use the pulse current post-processing method to regulate the microstructure and mechanical properties of selective laser melted IN718 alloy. By subjecting the formed sample to pulse current treatment, the internal dislocation distribution is improved, the metal recrystallization is promoted, and the grains are refined. In order to obtain a selective laser melted IN718 alloy with better mechanical properties. On the other hand, the pulse current treatment takes a short time and significantly reduces energy consumption, thereby achieving the purpose of energy saving. The present invention provides new ideas and methods for preparing high-performance selective laser melted IN718 alloy parts.
[0005] A pulse current rapid post-processing method for improving the tensile properties of IN718 alloy produced by selective laser melting is disclosed: an IN718 alloy sample produced by selective laser melting is cut from a substrate and the surface is polished to be smooth; a pulse current device is clamped at both ends of the IN718 alloy sample and pulse current treatment is performed, the Joule heating effect of the pulse current is used to promote the movement of atoms and dislocations inside the sample, and the non-thermal effect of the pulse current is used to promote recrystallization, thereby improving the tensile properties of the IN718 alloy sample.
[0006] Furthermore, the IN718 alloy sample is a rectangular parallelepiped, and the pulse current device is clamped on two opposite sides of the IN718 alloy sample with the smallest area.
[0007] Furthermore, the pulse current treatment is specifically as follows: the pulse frequency is 250-450 Hz, the pulse voltage is 30-90 V, the pulse current treatment time is 10-90 seconds, and after the pulse current treatment is completed, the IN718 alloy sample is naturally cooled in the air.
[0008] Furthermore, the method for manufacturing the IN718 alloy sample by selective laser melting is:
[0009] S1. Powder and pretreatment: prepare 18.3-19.8% Cr, 17.9-19.1% Fe, 5.4-6.2% Nb, 2.9-3.3% Mo, 0.81-0.93% Ti, 0.59-0.67% Al, 0.28-0.35% Mn, 0.04-0.06% C and the balance Ni by mass percentage, sieve the powder and dry at 90-100°C for 3-4h;
[0010] S2. Additive manufacturing: The selective laser melting equipment was evacuated and filled with protective gas. The forming platform temperature was 40-80°C. The laser power range was set to 200-360W, the scanning speed range was set to 890-1120mm / s, the scanning spacing was 75-85μm, the spot size was 70-80μm, the layer thickness was 25-50μm, and the IN718 alloy sample was prepared using a chessboard scanning strategy.
[0011] The beneficial effects of the present invention are:
[0012] The present invention utilizes the non-thermal effect of pulse current and the Joule thermal effect to perform pulse current treatment on the selective laser melted IN718 alloy, improve the internal dislocation distribution, promote metal recrystallization, and refine the grains, so that the plasticity of the IN718 alloy is greatly improved after the short-time pulse current treatment. At the same time, the pulse current treatment takes a short time and significantly reduces energy consumption, thereby achieving the purpose of energy conservation. The present invention successfully achieves the regulation of the structure and performance of the selective laser melted nickel-based high-temperature alloy through the "additive manufacturing + pulse current short-time post-treatment" method, which can provide certain theoretical guidance for the application of nickel-based high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Schematic diagram of pulse current treatment of selective laser melting of IN718 alloy in the present invention.
[0014] Figure 2 The microstructure metallographic diagram of the alloy in the deposited state and after pulse current treatment of the present invention
[0015] Figure 3 These are SEM photos of IN718 alloy before and after pulse current treatment according to the present invention.
[0016] Figure 4 This is a tensile stress-strain curve of the IN718 alloy sample before and after the pulse current of the present invention. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with the accompanying drawings.
[0018] The purpose of the present invention is to develop a pulse current rapid post-processing method for improving the tensile properties of IN718 alloy subjected to selective laser melting, so that the mechanical properties of IN718 alloy can be greatly improved under short-time pulse current treatment.
[0019] First, IN718 alloy samples were manufactured by selective laser melting. The specific steps are as follows:
[0020] S1. Powder and pretreatment: prepare 18.3-19.8% Cr, 17.9-19.1% Fe, 5.4-6.2% Nb, 2.9-3.3% Mo, 0.81-0.93% Ti, 0.59-0.67% Al, 0.28-0.35% Mn, 0.04-0.06% C and the balance Ni by mass percentage, sieve the powder and dry at 90-100°C for 3-4h;
[0021] S2. Additive manufacturing: The selective laser melting equipment was evacuated and filled with protective gas. The forming platform temperature was 40-80°C. The laser power range was set to 200-360W, the scanning speed range was set to 890-1120mm / s, the scanning spacing was 75-85μm, the spot size was 70-80μm, the layer thickness was 25-50μm, and the IN718 alloy sample was prepared using a chessboard scanning strategy.
[0022] The formed alloy was cut by wire cutting, and the sample surface pattern was polished smooth by a pre-grinder; the copper metal chuck of the pulse current device was clamped at the left and right ends of the IN718 alloy sample, and the pulse frequency was set to 250-450Hz, the pulse voltage was 30-90V, and the pulse current treatment was performed for 10-90 seconds. After the treatment, the IN718 alloy sample was naturally cooled in the air. The Joule heating effect of the pulse current was used to promote the movement of atoms and dislocations inside the sample, and the non-thermal effect of the pulse current was used to promote recrystallization, thereby improving the tensile properties of the IN718 alloy sample.
[0023] Embodiment 1:
[0024] In this embodiment, a nickel-based high-temperature alloy with excellent mechanical properties was obtained after different voltage pulse current treatments at a frequency of 350 Hz and a time of 60 seconds. The improvement of mechanical properties is achieved through grain refinement, and its coarse columnar crystals are transformed into fine equiaxed grains after experiencing pulse current.
[0025] S1. Powder and pretreatment: The powder is sieved and dried at 100°C for 4h according to the mass percentage of 19.6% Cr, 18.7% Fe, 5.8% Nb, 3.2% Mo, 0.87% Ti, 0.66% Al, 0.31% Mn, 0.043% C and the balance Ni;
[0026] S2, Additive Manufacturing: After vacuum treatment, the selective laser melting equipment was filled with argon gas, the forming platform temperature was 80°C, the laser power was set to 285W, the scanning speed was set to 960mm / s, the scanning spacing was 80μm, the spot size was 75μm, the layer thickness was 30μm, and the chessboard scanning strategy was used to prepare the sample;
[0027] S3, pretreatment of alloy: cut the formed alloy by wire cutting, and grind the sample surface to smoothness by pre-grinding machine;
[0028] S4. Pulse current treatment: Clamp the prepared alloy on a copper metal chuck, set the pulse frequency to 350Hz, increase the pulse voltage to 50V, 70V, and perform pulse current treatment for 60 seconds. After the treatment, the alloy is naturally cooled in the air.
[0029] The pulse current schematic diagram of the present invention is as follows Figure 1 After the prepared sample is clamped in a copper metal chuck, a certain voltage is adjusted to carry out pulse current treatment for a suitable time. After the treatment is completed, the sample is removed after natural cooling.
[0030] The microstructure of IN718 deposited by SLM and treated by pulse current is shown in the following figure: Figure 2 As shown, (a) is a metallographic photograph of the deposited IN718 alloy, (b) is a metallographic photograph of the IN718 alloy after 50V60s pulse current treatment, (c) and (d) are metallographic photographs of the IN718 alloy after 70V60s pulse current treatment. Figure 2 In (a), it can be seen that the deposited IN718 presents a layered molten pool shape, and the columnar crystals grow along the deposition direction, that is, the temperature gradient direction. The layered structure molten pool can still be observed under the 50V60s parameter, and the pulse current treatment with a lower voltage will not change this structure. During the pulse current treatment of the same time, as the pulse current and voltage increase, the columnar crystals first transform into refined subgrains, and then recrystallize and transform into refined equiaxed grains. The deposited state has a large columnar crystal size, with the maximum and minimum sizes of 134.2μm and 36.1μm, respectively. After 50V60s pulse current treatment, the elongated subgrains are smaller in size, with an average width of 40.8μm. Recrystallization occurs after 70V60s EPT, and a large number of columnar crystals are transformed into equiaxed crystals, with an average grain size of 45.5μm.
[0031] The SEM photos before and after the pulse current treatment of the present invention are as follows Figure 3 As shown, (a) and (d) are deposited IN718, (b) and (e) are IN718 after 50V 60s pulse current treatment, (c) and (f) are IN718 after 70V 60s pulse current treatment. SLM deposited sample ( Figure 3 In (a) and (d)), columnar dendrites and cellular substructures can be observed. The growth direction of the dendrites depends on the heat flow direction. The heat flow direction of the selective laser melting is the forming direction. When the pulse voltage is 50V, some columnar crystals become equiaxed crystals. When the pulse voltage is 70V ( Figure 3 In (c) and (f), the temperature increase causes the substructure to completely disappear and a large number of equiaxed crystals appear.
[0032] The tensile stress-strain curves of IN718 alloy before and after pulse current treatment of the present invention are as follows: Figure 4 As shown in the figure, under the same processing time of 60s, with the increase of voltage, the tensile strength first increases and then decreases, and the plasticity gradually increases. After the 50V60s pulse current treatment, the tensile strength reaches the maximum value, the tensile strength is 1151±6MPa, and the elongation is 21.4±1.2%. Compared with the deposited sample, the tensile strength is increased by about 3.8%, the elongation is increased by about 43.6%, and the strength and plasticity are improved. After the 70V60s pulse current treatment, the elongation reaches the maximum value of 26±3.3%, which is about 74.5% higher than the deposited IN718, and the plasticity is significantly improved. The pulse current promotes recrystallization inside the sample and promotes grain refinement. According to the Hall-Petch relationship, it can effectively improve the strength and plasticity of the sample. The non-thermal effect and the Joule thermal effect work together to promote the movement of dislocations inside the sample, making the dislocations evenly distributed and improving the plasticity of the sample. After the 50V60s pulse current treatment, the strengthening phases γ′ and γ″ increase, providing additional strength to the sample. Under the coupling effect, the tensile strength is improved, and a large number of columnar crystals are transformed into fine subgrains, and some recrystallized into fine equiaxed crystals, so the plasticity is also greatly improved. After the 70V60s pulse current treatment, the internal dislocations are evenly distributed, and a large number of columnar crystals are recrystallized and refined into equiaxed crystals, which greatly improves the plasticity, but the strength decreases. In addition to the influence of recrystallization, the magnetic field generated by the pulse current treatment also has a partial influence on the improvement of plasticity, that is, magneto-plasticity. The influence of the magnetic field on the plasticity of the metal mainly has two aspects: increasing the electronic damping of dislocations in the crystal and promoting the depinning of dislocations from paramagnetic barriers. In summary, pulse current treatment can achieve performance changes in a shorter time by appropriately adjusting parameters.
[0033] In summary, the present invention provides a pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy, which utilizes the non-thermal effect of pulse current and the Joule thermal effect to cause rapid recrystallization in a short time, and the plasticity of the alloy is greatly improved after short-time pulse current treatment. The present invention successfully achieves the regulation of the structure and properties of the selective laser melted nickel-based high-temperature alloy through the "additive manufacturing + pulse current short-time post-processing" method, which can provide certain theoretical guidance for the application of nickel-based high-temperature alloys.
[0034] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy, characterized in that: The IN718 alloy sample manufactured by selective laser melting was cut from the substrate and the surface was polished smooth. The pulse current device was clamped at both ends of the IN718 alloy sample and pulse current treatment was performed. The Joule heating effect of the pulse current was used to promote the movement of atoms and dislocations inside the sample, and the non-thermal effect of the pulse current was used to promote recrystallization, thereby improving the tensile properties of the IN718 alloy sample.
2. The pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy according to claim 1, characterized in that: The IN718 alloy sample is a rectangular parallelepiped, and the pulse current device is clamped on two opposite sides of the IN718 alloy sample with the smallest area.
3. The pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy according to claim 1, characterized in that: The pulse current treatment is specifically as follows: the pulse frequency is 250-450 Hz, the pulse voltage is 30-90 V, the pulse current treatment time is 10-90 seconds, and after the pulse current treatment is completed, the IN718 alloy sample is naturally cooled in the air.
4. The pulse current rapid post-processing method for improving the tensile properties of selective laser melted IN718 alloy according to claim 1, characterized in that: The method for manufacturing the IN718 alloy sample by selective laser melting is: S1. Powder and pretreatment: prepare 18.3-19.8% Cr, 17.9-19.1% Fe, 5.4-6.2% Nb, 2.9-3.3% Mo, 0.81-0.93% Ti, 0.59-0.67% Al, 0.28-0.35% Mn, 0.04-0.06% C and the balance Ni by mass percentage, sieve the powder and dry at 90-100°C for 3-4h; S2. Additive manufacturing: The selective laser melting equipment was evacuated and filled with protective gas. The forming platform temperature was 40-80°C. The laser power range was set to 200-360W, the scanning speed range was set to 890-1120mm / s, the scanning spacing was 75-85μm, the spot size was 70-80μm, the layer thickness was 25-50μm, and the IN718 alloy sample was prepared using a chessboard scanning strategy.
Citation Information
Cited By
Method for eliminating residual stress in additive manufacturing of nickel-based superalloy
CN119501101A