Micro-arc oxidation coating based on soft spark discharge and preparation method
Through micro-arc oxidation technology based on soft spark discharge, the problem of insufficient coating thickness on the surface of multi-principal alloys is solved, thickness-controllable coating preparation is achieved, wear resistance and biocompatibility are significantly improved, and it is suitable for biological applications. Medical materials.
Patent Information
- Application Number
- CN202411166774.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-25
AI Technical Summary
The thickness of the micro-arc oxidation coating prepared on the surface of the multi-principal alloy using the existing technology is relatively thin, resulting in limited improvement in wear resistance, film-base adhesion, corrosion resistance and biocompatibility.
Using micro-arc oxidation technology based on soft spark discharge, by adjusting the current density, current frequency and electrolyte composition, the coating thickness is controlled between 10 and 455 microns, forming a porous structure and micro-nano pores to improve the wear resistance and wear resistance of the coating. Biocompatibility.
The wear resistance, corrosion resistance and biocompatibility of the multi-principal element alloy are significantly improved. The coating thickness is controllable, the wear rate and corrosion current density are within an appropriate range, and it is suitable for biomedical materials.
Smart Images

Figure CN118835296A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of multi-principal alloy surface treatment, and in particular to a coating preparation method using a micro-arc oxidation technology based on soft spark discharge. Background Art
[0002] In recent years, multi-principal alloys have attracted extensive attention in the biomedical field due to their advantages such as high strength / hardness, high fracture toughness and excellent corrosion resistance. Multi-principal alloys of the TiNbZr system are superior to pure titanium and titanium alloys in terms of biocompatibility, mechanical properties and corrosion resistance, and can be used as a new generation of medical metal materials with superior overall performance.
[0003] The service environment of orthopedic implants in the human body is relatively complex. The good stability of implants in bones depends not only on the performance of the matrix material, but also on the physical and chemical properties of its surface. In order to meet the requirements of biomedical applications, the wear resistance, corrosion resistance and biocompatibility of the surface of multi-principal alloys still need to be further improved. Surface modification is an effective way to improve the surface properties of metal materials (wear resistance, corrosion resistance and biocompatibility). Micro-arc oxidation (MAO) is an electrochemical surface modification technology that can prepare oxide ceramic coatings on the surface of valve metals. The micro-arc oxidation coating is metallurgically bonded to the substrate, and the coating has a strong bonding force with the metal substrate. The coating prepared by conventional micro-arc oxidation has a double-layer structure, with a loose and porous outer layer and a dense but thin inner layer. In addition, spark discharge is continuously generated during the micro-arc oxidation process, leaving many discharge channels in the coating. The corrosive medium will invade the substrate through these channels, which has a very limited effect on the improvement of the corrosion resistance of the coating. Soft spark discharge is a unique phenomenon in the micro-arc oxidation process. When the applied cathode (negative) current is higher than the anode (positive) current, a soft spark transition may occur during the micro-arc discharge process. In micro-arc oxidation based on soft spark discharge, the forward voltage drops sharply after rising for a period of time during the treatment process, accompanied by a decrease in acousto-optic emission, and the sparks tend to be evenly distributed on the sample surface. This voltage drop weakens the spark intensity and avoids the negative impact of the increasing spark intensity on the coating during conventional micro-arc oxidation. Therefore, a thicker, more uniform and dense oxide coating can be produced on the metal surface. Compared with conventional micro-arc oxidation coatings, the coatings prepared by micro-arc oxidation based on soft spark discharge have smaller roughness and pore size on the outer layer, fewer discharge channels, and a thicker and denser inner layer, which can significantly improve the corrosion resistance and wear resistance of the alloy.
[0004] It is known from existing research reports that dense coatings can be produced on the surfaces of aluminum and magnesium alloys by micro-arc oxidation based on soft spark discharge, but it has not been very successful on titanium alloys. The coating thickness prepared on the surface of multi-principal alloys of the TiNbZr system by conventional micro-arc oxidation is relatively thin, only a few microns, and its performance still has a lot of room for improvement. The micro-arc oxidation technology based on soft spark discharge in the present invention can be used to prepare coatings with controllable thickness, and can greatly improve the wear resistance, corrosion resistance and biocompatibility of multi-principal alloys to meet biomedical requirements. This research has broad application prospects and academic research value, and is expected to generate greater social value and economic benefits. Summary of the invention
[0005] The present invention designs and develops a method for preparing a coating on the surface of a multi-principal alloy using a micro-arc oxidation technology based on soft spark discharge, which adopts a special micro-arc oxidation preparation method. One of the inventive purposes of the present invention is to solve the problem that the micro-arc oxidation coating prepared on the surface of a multi-principal alloy by the existing preparation method is relatively thin, and the improvement of the coating's wear resistance, film-base bonding, corrosion resistance, and biocompatibility is relatively limited. The preparation method of the present invention has a simple process, low cost, and excellent film performance, and is suitable for industrial production.
[0006] The second purpose of the present invention is to provide a multi-principal alloy micro-arc oxidation film layer, which is composed of micro-nano-scale holes and has a controllable thickness, strong film bonding, excellent wear resistance and biocompatibility. The micro-arc oxidation film layer of the present invention enhances the mechanical bonding ability between tissue cells and implants, and the micro-nano structure on the surface is conducive to the attachment and growth of new bone. The excellent bonding force, wear resistance and corrosion resistance can meet the needs of clinical operations and long-term service.
[0007] To achieve the above purpose, the thickness of a micro-arc oxidation coating based on soft spark discharge of the present invention is in the range of 10 to 455 microns and can be controlled and adjusted; the wear rate of the micro-arc oxidation coating is 1×10 -5 ~3×10 -4 mm 3 ·N -1 ·m -1 The corrosion current density of the micro-arc oxidation coating is 1×10 -10 ~5×10 -8 A / cm 2 The coating has good biocompatibility and is conducive to the attachment and growth of bone cells.
[0008] The invention discloses a micro-arc oxidation coating based on soft spark discharge, comprising a substrate and a coating generated on the surface of the substrate by micro-arc oxidation; the substrate is an alloy containing Ti, Nb and Zr; the coating generated on the surface of the substrate by micro-arc oxidation has a porous structure, and is distributed with micro-nano-scale holes and / or groove-shaped holes; spherical particles are also distributed on the surface of the coating; among the micro-nano-scale holes, the pore diameter of the micron-scale holes is 1 to 10 microns; the particle diameter of the spherical particles is 0.5 to 2 microns; the length of the groove-shaped holes is 10 to 50 microns, and the porosity of the coating generated on the surface of the substrate by micro-arc oxidation is 3% to 30%.
[0009] The present invention discloses a micro-arc oxidation coating based on soft spark discharge, wherein the coating is formed on the surface of a substrate by micro-arc oxidation, and the thickness thereof is 10 to 455 microns; the wear rate of the coating is 1×10 -5 ~3×10 -4 mm 3 ·N -1 ·m -1 The corrosion current density of the micro-arc oxidation coating in PBS solution is 1×10 -10 ~5×10 -8 A / cm 2 .
[0010] The invention provides a micro-arc oxidation coating based on soft spark discharge, and the coating has biocompatibility.
[0011] Preferably, in the micro-arc oxidation coating based on soft spark discharge of the present invention, the molar ratio of Ti, Nb and Zr in the substrate is 0.8-1.2:0.8-1.2:0.8-1.2, preferably 1:1:1.
[0012] The multi-principal-element matrix alloy of the TiNbZr system designed and selected by the present invention is superior to pure titanium and titanium alloy in terms of biocompatibility, mechanical properties and corrosion resistance.
[0013] The present invention discloses a method for preparing a micro-arc oxidation coating based on soft spark discharge, comprising the following steps:
[0014] A substrate with a clean and dry surface is used as an anode, and stainless steel is used as a cathode; the anode and the cathode are placed in a micro-arc oxidation electrolyte to perform micro-arc oxidation to obtain a micro-arc oxidation coating on the substrate; the substrate is a multi-principal alloy containing Ti, Nb, and Zr; the micro-arc oxidation electrolyte comprises a main salt, a compounding agent, and deionized water; wherein the main salt is selected from at least one of sodium silicate and sodium phosphate; the compounding agent is selected from at least one of sodium hydroxide and potassium hydroxide; in the arc oxidation electrolyte, the concentration of the main salt is 20-105 g / L;
[0015] During micro-arc oxidation, control the current density of the forward current to be 50-500 mA / cm 2 , the current density of negative current is 80~2000mA / cm 2 , and the negative current density is greater than the positive current density, the duty cycle is 5% to 30%, the pulse frequency is 100 to 1000 Hz, the time is 5 to 60 minutes, and the temperature is 20 to 40°C.
[0016] When used in industry, the matrix material is prepared by melting a certain proportion of pure metal particles of the TiNbZr system by vacuum arc melting or vacuum induction melting to obtain a medium / high entropy alloy button ingot of the system. Then it is cut to obtain an object of set size and morphology; then the surface of the object is pretreated, the surface is polished with sandpaper, and degreased and cleaned to obtain a clean and dry sample.
[0017] When used in industry, the inert material may be one of the conductive materials such as stainless steel and graphite.
[0018] The invention discloses a method for preparing a micro-arc oxidation coating based on soft spark discharge, wherein the micro-arc oxidation electrolyte is an alkaline electrolyte.
[0019] Preferably, the present invention provides a method for preparing a micro-arc oxidation coating based on soft spark discharge, wherein the concentration of the main salt in the micro-arc oxidation electrolyte is 20 to 105 g / L. In the present invention, the amount of sodium silicate in the main salt is greater than 20 g / L because in the micro-arc oxidation process system developed by the present invention, it can not only improve the conductivity of the solution, but also provide reasonable and sufficient silicate ions for micro-arc oxidation treatment. If the concentration of sodium silicate is too low, the voltage increase in the constant current mode will be very slow, the processing time will be too long, and it will be difficult to provide sufficient silicate ions for micro-arc oxidation treatment.
[0020] Preferably, in the micro-arc oxidation electrolyte, the concentration of the compounding agent is 2 to 20 g / L, preferably 2 to 10 g / L, and more preferably 6 to 10 g / L.
[0021] Preferably, the density of the negative current is greater than the density of the positive current.
[0022] As a further preferred embodiment, the current density of the forward current is 180 to 220 mA / cm 2 At this time, the current density of the negative current is 300~1000mA / cm 2 , preferably 800~1000mA / cm 2 or 300~400mA / cm 2 In the present invention, the density of the negative current is controlled to be greater than the density of the positive current and the current density of the negative current is increased by 300-1000 mA / cm 2This is because the negative current density required for the TiNbZr system multi-principal alloy to enter the soft spark discharge transition is greater than that of Al, Mg, and Ti. As a preferred embodiment, the negative current density / positive current density in the present invention is greater than or equal to 2.3, so that the soft spark discharge transition can occur more stably during the micro-arc oxidation process.
[0023] Preferably, a constant current mode is adopted during micro-arc oxidation.
[0024] As a further preference, when the electrolyte comprises:
[0025] The concentration of main salt sodium silicate is 24-26g / L, the concentration of sodium phosphate is 9-11g / L; the concentration of compounding agent sodium hydroxide is 7-9g / L;
[0026] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 60min, temperature 25℃, a coating with a thickness of 440-455 microns can be obtained.
[0027] The wear rate of the coating is (2.4~2.45)×10 -4 mm 3 ·N -1 ·m -1 .
[0028] As a further preference, when the electrolyte comprises:
[0029] The concentration of the main salt sodium silicate is 27-29g / L; the concentration of the compounding agent sodium hydroxide is 7-9g / L;
[0030] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 780~820mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 15min, temperature 25℃; a coating with a thickness of 25 to 38 microns can be obtained.
[0031] The wear rate of the coating is (7.15~7.25)×10 -5 mm 3 ·N -1 ·m -1 .
[0032] As a further preference, when the electrolyte comprises:
[0033] The concentration of the main salt sodium phosphate is 24-26g / L; the concentration of the compounding agent sodium hydroxide is 7-9g / L;
[0034] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 20%, pulse frequency 200Hz, time 45min, temperature 40℃; a coating with a thickness of 118 to 125 microns can be obtained,
[0035] The wear rate of the coating is (1.15~1.2)×10 -4 mm 3 ·N -1 ·m -1 .
[0036] As a further preference, when the electrolyte comprises:
[0037] The concentration of the main salt sodium silicate is 24-26g / L; the concentration of the compounding agent sodium hydroxide is 1.8-2.2g / L, and the concentration of potassium hydroxide is 1.8-2.2g / L;
[0038] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 20%, pulse frequency 1000Hz, time 45min, temperature 40℃; coating with thickness of more than 200 microns can be obtained;
[0039] The wear rate of the coating is (8.4~8.45)×10 -5 mm 3 ·N -1 ·m -1 .
[0040] It can be seen that by optimizing the composition of the electrolyte and increasing the pulse frequency, the coating thickness can be quickly increased in a short time, and the wear rate of the coating is also significantly reduced.
[0041] Beneficial effects: The micro-arc oxidation coating and preparation method of the present invention have the following advantages:
[0042] (1) The present invention uses a micro-arc oxidation technology based on soft spark discharge to treat the sample surface. The surface of the obtained oxide coating presents a porous structure with multiple micro-nano pores distributed thereon. There are also many spherical particles on the surface of the oxide coating. The pore size of the micron-sized pores is 1 to 10 microns, and there are many nano-sized pores on the coating surface. The spherical particle size is 0.5 to 2 microns, and the porosity ranges from 3% to 30%. The unique micro-nano morphology formed by the oxide film layer of the present invention has good hydrophilicity, which is conducive to the attachment and growth of bone tissue and improves the bone bonding ability.
[0043] (2) The preparation method of a micro-arc oxidation coating based on soft spark discharge of the present invention adopts a compounding agent to regulate the ion concentration of the electrolyte, the electrolyte conductivity and the spark discharge intensity during the micro-arc oxidation process. Coatings of different thicknesses can be obtained according to the regulation of the electrolyte and electrical process parameters, and the thickness can even reach 455 microns. This solves the problem that the micro-arc oxidation coating prepared on the surface of the multi-principal alloy by the existing preparation method is relatively thin, and the improvement of the wear resistance, membrane-base bonding and corrosion resistance and biocompatibility of the coating is relatively limited.
[0044] (3) The thickness of the micro-arc oxidation coating based on soft spark discharge of the present invention can be controlled and adjusted according to needs, and the thickness range is: 10 to 455 microns; the wear resistance, corrosion resistance and biocompatibility of the micro-arc oxidation coating based on soft spark discharge of the present invention are greatly improved, and the wear rate of the micro-arc oxidation coating is 1×10 -6 ~2.5×10 - 4 mm 3 ·N -1 ·m -1 , after optimization, it can be as low as 1×10 -6 ~8.5×10 -5 mm 3 ·N -1 ·m -1 ; The corrosion current density of the micro-arc oxidation coating is 1×10 -10 ~5×10 -8 A / cm 2 The coating has good biocompatibility and is conducive to the attachment and growth of bone cells. The coating has good stability and safety.
[0045] (4) The present invention provides a relatively precise parameter range for the micro-arc oxidation process, such as current density, current frequency, duty cycle and reaction time, which can achieve fine control of the micro-arc oxidation process and ensure the uniformity and consistency of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solution of the present invention, the drawings required for use in the embodiments or technical descriptions will be briefly introduced below. The drawings described below are only some embodiments of the present invention.
[0047] Figure 1 This is a SEM image of the surface morphology of a coating prepared by micro-arc oxidation technology based on soft spark discharge provided in Example 1 of the present invention.
[0048] Figure 2 This is a surface morphology SEM image of a coating prepared on the surface of a medium entropy alloy provided in Example 2 of the present invention using a micro-arc oxidation technology based on soft spark discharge.
[0049] Figure 3 This is a surface morphology SEM image of a coating prepared on the surface of a multi-principal alloy provided in Example 3 of the present invention using a micro-arc oxidation technology based on soft spark discharge.
[0050] Figure 4 This is a surface energy spectrum of a coating prepared by micro-arc oxidation technology based on soft spark discharge, provided in one embodiment of the present invention.
[0051] Figure 5 This is a SEM image of the cross-sectional morphology of a coating prepared by micro-arc oxidation technology based on soft spark discharge provided in Example 1 of the present invention.
[0052] Figure 6 The figure is a SEM image of the cross-sectional morphology of a micro-arc oxidation coating according to an embodiment of the present invention.
[0053] Figure 7 This is a cross-sectional SEM image of a coating prepared on the surface of a medium-entropy alloy provided in Example 2 of the present invention using a micro-arc oxidation technology based on soft spark discharge.
[0054] Figure 8 The voltage-time curves of four embodiments of the present invention during the process of preparing coatings using micro-arc oxidation technology based on soft spark discharge.
[0055] Fig. 9 This is a SEM image of the wear scar morphology of Example 2 of the present invention after dry friction for 30 minutes under a load of 5N.
[0056] Fig.10 It is an optical three-dimensional contour diagram of the wear scar of another embodiment of the present invention after dry friction for 30 minutes under a load of 5N.
[0057] Fig.11 This is a dynamic point polarization curve diagram of Example 2 of the present invention in PBS simulated human body fluid.
[0058] Fig.12This is a SEM image of cells attached to a micro-arc oxidation coating sample provided by another embodiment of the present invention for 2 hours.
[0059] Fig.13 It is a cross-sectional SEM image of the coating obtained by conventional micro-arc oxidation technology in Comparative Example 1 of the present invention.
[0060] Fig.14 It is a SEM image of the cross-sectional morphology of the coating provided in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0061] The present invention will be further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0062] Sample pretreatment: The multi-principal alloy button ingots of the system were smelted, and then wire-cut, and then the surface was polished with sandpaper, and degreased and cleaned to obtain a clean and dry sample. After micro-arc oxidation, deionized water was used for ultrasonic cleaning and drying to obtain a micro-arc oxidation coating.
[0063] The invention provides an electrolyte for micro-arc oxidation, wherein the main salt is one of sodium silicate and sodium phosphate or a combination thereof in a certain proportion; and the compounding agent is one or more of sodium hydroxide and potassium hydroxide.
[0064] The concentration of the main salt is 20-105 g / L, and the concentration of a single component in the compound is 2-20 g / L.
[0065] The present invention provides a method for preparing a micro-arc oxidation coating based on soft spark discharge, wherein the process parameters are: a constant current power supply mode is adopted, and the current density of the forward current is 50-500 mA / cm 2 , the current density of negative current is 50~2000mA / cm 2 , duty cycle 5%~30%, pulse frequency 100~1000Hz, time 5~60min, temperature 20~40℃.
[0066] Test Method
[0067] Surface / cross-section morphology and element content test: The surface and cross-section morphology of the samples were characterized using a scanning electron microscope (SEM, HeliosNanolab G3 UC, Czech Republic) equipped with EDS, secondary electron and backscattered electron mode, 20Kv.
[0068] Friction and wear test: The friction test was conducted using a ball-on-disc high-temperature friction and wear tester (Zhongke Kaihua HT-1000) with a load of 5N and a rotation speed of 120r / min. The grinding material used was a Si3N4 ceramic ball with a radius of 2mm, and the test lasted for 30min. After friction, the wear marks and the amount of wear were analyzed using SEM and an optical profiler (Veeco Metrology Inc WYKO NT9100, USA).
[0069] The pore size, porosity, coating thickness, etc. of the oxide film layer are calculated using Image Pro software.
[0070] Example 1
[0071] Step 1: The TiNbZr pure metal particles with equal atomic ratios are melted by vacuum arc to obtain a medium entropy alloy button ingot. Then, the ingot is cut into a disc with a diameter of 20 mm and a thickness of 1.2 mm. The ingot is ultrasonically cleaned in acetone and anhydrous ethanol in turn, and then polished with 80#, 320#, 800#, and 1200# sandpaper in stages, ultrasonically treated in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0072] Step 2, prepare electrolyte: the concentration of main salt sodium silicate is 25g / L, the concentration of sodium phosphate is 10g / L; the concentration of compounding agent sodium hydroxide is 8g / L; after mixing, the volume is adjusted to 2L, and stirred evenly with a stirring device.
[0073] Step 3: Micro-arc oxidation
[0074] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 400mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 60min, temperature 25℃.
[0075] Step 4: After micro-arc oxidation, wait until the voltage drops to 0 V, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in turn, and then dry it in air.
[0076] The ceramic coating prepared by the above-mentioned micro-arc oxidation technical parameters, the surface morphology of the coating of Example 1 is shown in the attached Figure 1 The coating surface is porous and has spherical silica particles, with an average porosity of 5.26%. Figure 5 The coating thickness is 450 microns. Figure 8 (Left, TiNbZr) is the voltage-time curve of Example 1 during the micro-arc oxidation process. During the micro-arc oxidation process, a voltage drop occurred, resulting in a decrease in the spark discharge intensity, that is, a soft spark discharge phenomenon occurred. The wear rate of the sample surface in Example 1 is 2.43×10-4 mm 3 ·N -1 ·m -1 . Fig.12 This is a SEM image of cells attached to a micro-arc oxidation coating sample provided by another embodiment of the present invention for 2 hours. The coating has good biocompatibility, bone cells can be well attached to the coating surface, and pseudopodia can penetrate deep into the micro-nano pores, effectively improving the bone bonding ability.
[0077] Example 2
[0078] Step 1: The TiNbZr pure metal particles with equal atomic ratios are melted by vacuum arc to obtain a medium entropy alloy button ingot. Then, the ingot is cut into a disc with a diameter of 20 mm and a thickness of 1.2 mm. The ingot is ultrasonically cleaned in acetone and anhydrous ethanol in turn, and then polished with 80#, 320#, 800#, and 1200# sandpaper in stages, ultrasonically treated in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0079] Step 2, prepare electrolyte: the concentration of main salt sodium silicate is 28.4g / L; the concentration of compounding agent sodium hydroxide is 8g / L; after mixing, the volume is fixed to 2L, and stirred evenly with a stirring device.
[0080] Step 3: Micro-arc oxidation
[0081] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 800mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 15min, temperature 25℃.
[0082] Step 4: After micro-arc oxidation, wait until the voltage drops to 0 V, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in turn, and then dry it in air.
[0083] The ceramic coating prepared by the above-mentioned micro-arc oxidation technical parameters, the surface morphology of the coating of Example 2 is shown in the attached Figure 2 There are many micro-nano holes distributed on the surface, and there are many spherical particles on the surface, with a porosity of 10%. Figure 4 This is the surface energy spectrum of Example 2, the surface of which is mainly composed of metal oxides and silicon dioxide, containing a small amount of sodium salt. Figure 7 This is the cross-sectional morphology SEM image of Example 2, and the coating thickness is about 30 microns. Fig. 9 This is the SEM image of the wear scar morphology of Example 2 after dry friction for 30 minutes under a load of 5N. During the friction process, the wear debris will fill into the pores. The surface silica hardness is relatively high, the wear scar is relatively shallow, and the wear rate is 7.20×10 -5 mm 3·N -1 ·m -1 . Fig.10 This is an optical three-dimensional contour diagram of the wear scar of another embodiment after dry friction for 30 minutes under a load of 5N. It can also be seen that the wear scar is shallow, the wear amount is low, and the wear resistance is good. Fig.11 This is the dynamic point polarization curve of Example 2 of the present invention in PBS simulated human body fluid, and the corrosion current density is 2.26×10 -9 A / cm 2 The surface coating has good corrosion resistance.
[0084] Example 3
[0085] Step 1: Vacuum arc melting TiNbZr pure metal particles with equal atomic ratios to obtain high entropy alloy button ingots. Then wire cut into discs with a diameter of 20 mm and a thickness of 1.2 mm. Ultrasonic cleaning in acetone and anhydrous ethanol in turn, then polishing with 80#, 320#, 800#, and 1200# sandpaper step by step, ultrasonically in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0086] Step 2, prepare electrolyte: the concentration of main salt sodium phosphate is 25g / L; the concentration of compounding agent sodium hydroxide is 8g / L; after mixing, the volume is fixed to 2L and stirred evenly with a stirring device.
[0087] Step 3: Micro-arc oxidation
[0088] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 400mA / cm 2 , duty cycle 20%, pulse frequency 200Hz, time 45min, temperature 40℃.
[0089] Step 4: After micro-arc oxidation, wait until the voltage drops to 0 V, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in turn, and then dry it in air.
[0090] Figure 3 This is a SEM image of the surface morphology of the coating prepared on the surface of the high entropy alloy provided in Example 3 of the present invention using the micro-arc oxidation technology based on soft spark discharge. The surface shows a groove-like hole morphology. The coating thickness is about 120 microns. The wear rate is measured to be 1.17×10 -4 mm 3 ·N -1 ·m -1 The dynamic point polarization curve in PBS simulated human body fluid, the corrosion current density is 2.87×10 -8 A / cm 2
[0091] Example 4
[0092] Step 1: The TiNbZr pure metal particles with equal atomic ratios are melted by vacuum arc to obtain a medium entropy alloy button ingot. Then, the ingot is cut into a disc with a diameter of 20 mm and a thickness of 1.2 mm. The ingot is ultrasonically cleaned in acetone and anhydrous ethanol in turn, and then polished with 80#, 320#, 800#, and 1200# sandpaper in stages, ultrasonically treated in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0093] Step 2, prepare electrolyte: the concentration of main salt sodium silicate is 25g / L; the concentration of compounding agent sodium hydroxide is 2g / L, the concentration of potassium hydroxide is 2g / L, after mixing, the volume is fixed to 2L, and stirred evenly with a stirring device.
[0094] Step 3: Micro-arc oxidation
[0095] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 400mA / cm 2 , duty cycle 20%, pulse frequency 1000Hz, time 45min, temperature 40℃.
[0096] Step 4: After micro-arc oxidation, wait until the voltage drops to 0 V, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in turn, and then dry it in air.
[0097] Figure 6 This is a SEM image of the cross-sectional morphology of the micro-arc oxidation coating of Example 4 of the present invention. The cross-sectional area of the coating is uniform and dense, with a thickness of more than 200 microns. The wear rate is measured to be 8.43×10 -5 mm 3 ·N -1 ·m -1 The dynamic point polarization curve in PBS simulated human body fluid, the corrosion current density is 5.27×10 -8 A / cm 2 The surface coating has good corrosion resistance.
[0098] Comparative Example 1
[0099] Step 1: The TiNbZr pure metal particles with equal atomic ratios are melted by vacuum arc to obtain a medium entropy alloy button ingot. Then, the ingot is cut into a disc with a diameter of 20 mm and a thickness of 1.2 mm. The ingot is ultrasonically cleaned in acetone and anhydrous ethanol in turn, and then polished with 80#, 320#, 800#, and 1200# sandpaper in stages, ultrasonically treated in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0100] Step 2, prepare electrolyte: the concentration of main salt sodium silicate is 25g / L; the concentration of compounding agent sodium hydroxide is 8g / L, mix and adjust the volume to 2L, and stir evenly with a stirring device.
[0101] Step 3: Micro-arc oxidation
[0102] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 0mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 45min, temperature 40℃.
[0103] Step 4: After micro-arc oxidation, wait until the voltage drops to 0 V, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in turn, and then dry it in air.
[0104] Fig.13 This is a SEM image of the cross-sectional morphology of the micro-arc oxidation coating of Comparative Example 1 of the present invention. The cross-sectional area of the coating is not uniform enough, and the thickness is less than 10 microns. The wear rate is measured to be 9.44×10 -4 mm 3 ·N -1 ·m -1 The dynamic point polarization curve in PBS simulated human body fluid, the corrosion current density is 6.29×10 -7 A / cm 2 It can be seen that in the absence of negative current, there is no voltage drop and soft spark discharge transition, which causes the coating to become uneven due to the gradually increasing voltage. In addition, the coating prepared by the conventional micro-arc oxidation method is thinner, resulting in the coating's wear resistance and corrosion resistance being worse than that of the coating prepared by micro-arc oxidation technology based on soft spark discharge.
[0105] Comparative Example 2
[0106] Step 1: The TiNbZr pure metal particles with equal atomic ratios are melted by vacuum arc to obtain a medium entropy alloy button ingot. Then, the ingot is cut into a disc with a diameter of 20 mm and a thickness of 1.2 mm. The ingot is ultrasonically cleaned in acetone and anhydrous ethanol in turn, and then polished with 80#, 320#, 800#, and 1200# sandpaper in stages, ultrasonically treated in anhydrous ethanol and deionized water for 5 minutes in turn, and air-dried for use.
[0107] Step 2, prepare electrolyte: the concentration of main salt sodium silicate is 25g / L; the concentration of compounding agent sodium hydroxide is 8g / L, mix and adjust the volume to 2L, and stir evenly with a stirring device.
[0108] Step 3: Micro-arc oxidation
[0109] The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of the negative current is 200mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 45min, temperature 40℃.
[0110] Step 4: After micro-arc oxidation, wait until the voltage drops to 0, remove the sample, and clean it with deionized water and anhydrous ethanol ultrasonically in sequence, and then dry it in air.
[0111] Fig.14 The cross-sectional morphology SEM image of the micro-arc oxidation coating of comparative example 2 of the present invention is shown in FIG. The coating thickness is less than 10 microns. The wear rate is measured to be 9.02×10 -4 mm 3 ·N -1 ·m -1 The dynamic point polarization curve in PBS simulated human body fluid, the corrosion current density is 5.18×10 -7 A / cm 2 It can be seen that under the condition of low negative current density, there is no voltage drop and soft spark discharge transition, and its thickness is not much different from that of the coating prepared by conventional micro-arc oxidation method, which leads to the coating's wear resistance and corrosion resistance being worse than that of the coating prepared by micro-arc oxidation technology based on soft spark discharge.
[0112] According to the above embodiments and Figures 1 to 14 The micro-arc oxidation coating based on soft spark discharge and the preparation method thereof of the present invention have the following advantages:
[0113] (1) The present invention uses a micro-arc oxidation technology based on soft spark discharge to treat the sample surface, and the obtained oxide coating surface presents a porous structure with multiple micro-nano holes distributed thereon, and there are also many spherical particles on the surface of the oxide coating. The unique micro-nano morphology formed by the oxide film layer of the present invention is conducive to the attachment and growth of bone tissue and improves the bone bonding ability.
[0114] (2) The preparation method of a micro-arc oxidation coating based on soft spark discharge of the present invention uses compounding agents and additives to regulate the ion concentration of the electrolyte, the electrolyte conductivity and the spark discharge intensity during the micro-arc oxidation process. Coatings of different thicknesses can be obtained according to the regulation of the electrolyte and electrical process parameters, and the thickness can even reach 455 microns. This solves the problem that the micro-arc oxidation coating prepared on the surface of a multi-principal alloy by the existing preparation method is relatively thin, and the improvement of the coating's wear resistance, membrane-base bonding, corrosion resistance and biocompatibility is relatively limited.
[0115] (3) The thickness of the micro-arc oxidation coating based on soft spark discharge of the present invention can be controlled and adjusted according to needs, and the thickness range is: 10 to 455 microns; the wear rate of the micro-arc oxidation coating is 1×10 -5 ~3×10 -4 mm 3 ·N -1 ·m -1 ; The corrosion current density of the micro-arc oxidation coating is 1×10 -10 ~5×10 -8 A / cm 2 The coating has good biocompatibility and is conducive to the attachment and growth of bone cells. The coating has good stability and safety. The wear resistance, corrosion resistance and biocompatibility of the micro-arc oxidation coating based on soft spark discharge of the present invention are greatly improved.
[0116] (4) The present invention provides a relatively precise parameter range for the micro-arc oxidation process, such as current density, current frequency, duty cycle and reaction time, which can achieve fine control of the micro-arc oxidation process and ensure the uniformity and consistency of the coating.
[0117] The above disclosures are only several embodiments of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A micro-arc oxidation coating based on soft spark discharge, characterized in that: It comprises a substrate and a coating formed on the surface of the substrate by micro-arc oxidation; the substrate is an alloy containing Ti, Nb and Zr; The coating generated by micro-arc oxidation on the surface of the substrate has a porous structure with distributed micro-nanoscale holes and / or groove-shaped holes; spherical particles are also distributed on the surface of the coating; among the micro-nanoscale holes, the pore size of the micron-scale holes is 1 to 10 microns; the particle size of the spherical particles is 0.5 to 2 microns; the length of the groove-shaped holes is 10 to 50 microns, and the porosity of the coating generated by micro-arc oxidation on the surface of the substrate is 3% to 30%.
2. The micro-arc oxidation coating based on soft spark discharge according to claim 1, characterized in that: The coating formed by micro-arc oxidation on the substrate surface has a thickness of 10 to 455 microns; the wear rate of the coating is 1×10 -5 ~3×10 - 4 mm 3 ·N -1 ·m -1 The corrosion current density of the micro-arc oxidation coating in PBS solution is 1×10 -10 ~5×10 -8 A / cm 2 .
3. The micro-arc oxidation coating based on soft spark discharge according to claim 1, characterized in that: The molar ratio of Ti, Nb and Zr in the matrix is 0.8-1.2:0.8-1.2:0.8-1.2, preferably 1:1:
1.
4. A method for preparing a micro-arc oxidation coating based on soft spark discharge as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: A substrate with a clean and dry surface is used as an anode, and an inert material is used as a cathode; the anode and the cathode are placed in a micro-arc oxidation electrolyte to perform micro-arc oxidation to obtain a micro-arc oxidation coating on the substrate; the substrate is a multi-principal alloy containing Ti, Nb, and Zr; the micro-arc oxidation electrolyte comprises a main salt, a compounding agent, and water; the main salt is selected from at least one of sodium silicate and sodium phosphate; the compounding agent is selected from at least one of sodium hydroxide and potassium hydroxide; in the arc oxidation electrolyte, the concentration of the main salt is 20-105 g / L; During micro-arc oxidation, control the current density of the forward current to be 50-500 mA / cm 2 , the current density of negative current is 80~2000mA / cm 2 , and the negative current density is greater than the positive current density, the duty cycle is 5% to 30%, the pulse frequency is 100 to 1000 Hz, the time is 5 to 60 minutes, and the temperature is 20 to 40°C.
5. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: The micro-arc oxidation electrolyte is an alkaline electrolyte; in the micro-arc oxidation electrolyte, the concentration of the main salt is 20-105 g / L, and the amount of sodium silicate in the main salt is preferably greater than 20 g / L.
6. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: In the micro-arc oxidation electrolyte, the concentration of the compounding agent is 2 to 20 g / L, preferably 2 to 10 g / L, and more preferably 6 to 10 g / L.
7. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: The current density of the forward current is 180~220mA / cm 2 At this time, the current density of the negative current is 300~1000mA / cm 2 , preferably 800~1000mA / cm 2 or 300~400mA / cm 2 .
8. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: During micro-arc oxidation, constant current mode is adopted.
9. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: When the electrolyte composition is: The concentration of the main salt sodium phosphate is 24-26g / L; the concentration of the compounding agent sodium hydroxide is 7-9g / L; The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 20%, pulse frequency 200Hz, time 45min, temperature 40℃; a coating with a thickness of 118 to 125 microns can be obtained, The wear rate of the coating is (1.15~1.2)×10 -4 mm 3 ·N -1 ·m -1 .
10. The method for preparing a micro-arc oxidation coating based on soft spark discharge according to claim 4, characterized in that: When the electrolyte composition is: The concentration of main salt sodium silicate is 24-26g / L, the concentration of sodium phosphate is 9-11g / L; the concentration of compounding agent sodium hydroxide is 7-9g / L; The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 60min, temperature 25℃, a coating with a thickness of 440-455μm was obtained, The wear rate of the coating is (2.4~2.45)×10 -4 mm 3 ·N -1 ·m -1 ; When the electrolyte composition is: The concentration of the main salt sodium silicate is 27-29g / L; the concentration of the compounding agent sodium hydroxide is 7-9g / L; The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 780~820mA / cm 2 , duty cycle 10%, pulse frequency 100Hz, time 15min, temperature 25℃; a coating with a thickness of 25 to 38 microns was obtained, The wear rate of the coating is (7.15~7.25)×10 -5 mm 3 ·N -1 ·m -1 ; When the electrolyte composition is: The concentration of the main salt sodium silicate is 24-26g / L; the concentration of the compounding agent sodium hydroxide is 1.8-2.2g / L, and the concentration of potassium hydroxide is 1.8-2.2g / L; The micro-arc oxidation process parameters are set as follows: constant current mode is adopted, and the current density of the forward current is 200mA / cm 2 , the current density of negative current is 380~420mA / cm 2 , duty cycle 20%, pulse frequency 1000Hz, time 45min, temperature 40℃; obtain a coating with a thickness of more than 200 microns; The wear rate of the coating is (8.4~8.45)×10 -5 mm 3 ·N -1 ·m -1 .
Citation Information
Cited By
SLM porous titanium alloy ternary co-doped composite coating and preparation method thereof
CN120587480A