Modified porous amorphous carbon negative electrode material as well as preparation method and application thereof

By modifying the core-shell structure of porous amorphous carbon anode materials and conductive carbon coating technology, the reversible capacity and stability problems of amorphous carbon materials in lithium-ion and sodium-ion batteries are solved, achieving efficient electrochemical performance and Environmental tolerance.

CN118841546APending Publication Date: 2024-10-25葛传长
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410880943.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing amorphous carbon anode materials have problems such as low reversible capacity, low first Coulombic efficiency, poor electronic conductivity and poor environmental stability during application, which limits their wide application in lithium-ion and sodium-ion batteries.

Method used

Modified porous amorphous carbon negative electrode material is used, and a core-shell structure is formed through a mixture of porous amorphous carbon doped with F element in the core and conductive carbon in the outer shell, optimizing pore size distribution and conductivity, combined with the doping and conductivity of fluorine element Carbon coating improves the reversible capacity and conductive properties of the material.

Benefits of technology

It achieves high reversible mass specific capacity, high first Coulombic efficiency and low-temperature high-rate charge-discharge cycle retention characteristics, and the material surface is inert, which significantly improves the stability and performance attenuation problems in the air environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841546A_ABST
    Figure CN118841546A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a modified porous amorphous carbon negative electrode material which is of a core-shell structure, the core takes porous amorphous carbon as a main component, the shell is a mixture of amorphous carbon and conductive carbon, and the modified porous amorphous carbon negative electrode material has micropores, mesopores and macropores, based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 5-40% of the total pore volume, the mesopores account for 15-70% of the total pore volume, and the macropores account for 10-50% of the total pore volume. The material disclosed by the invention is obtained by crushing a carbon-rich precursor to obtain carbon powder particles, doping an F element, performing chemical etching to form pores, and performing composite coating and carbonization on amorphous carbon and conductive carbon. The material provided by the invention has a special three-dimensional porous structure, mesopore and macropore structures provide rapid transmission channels for electrolyte ions, abundant micropore structures and heteroelement modification sites, so that the mass specific capacity of the material is improved, the adsorbability of the material can be reduced, and the problem of placement attenuation of the amorphous carbon material in air is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy storage materials and relates to a negative electrode material, in particular to a modified porous amorphous carbon negative electrode material with a special pore size distribution. Background Art

[0002] Secondary battery technology is an effective solution for the current economic and social solution to large-scale energy storage, achieving energy conversion and efficient use of renewable energy, alleviating resource scarcity and environmental problems caused by traditional energy consumption, and achieving sustainable social development. Among the current secondary battery technologies, lithium-ion batteries are the most mature and widely used in commercial applications, but due to the limitation of lithium resources, they cannot support the development of large-scale energy storage power sources in the future. Sodium, which is in the same main group as lithium, has similar chemical properties and electrode potentials. In addition, sodium has abundant crustal reserves and low refining costs. In recent years, it has received great attention worldwide, and the development of sodium-ion battery technology has become a hot topic in the current energy storage field.

[0003] The research and development of negative electrode materials is the key to the development of secondary battery technology. At present, commercial negative electrode materials are still mainly carbon materials. According to the degree of crystallization, carbon materials are divided into two categories: graphite carbon and amorphous carbon. Among them, carbon-based negative electrode materials, represented by graphite, are the main negative electrode materials for commercial lithium-ion batteries, but their theoretical specific capacity is only 372mAh / g, and the production process involves a high-temperature graphitization process. The manufacturing cost and energy consumption are high, which limits its further development. In addition, the theoretical interlayer spacing of graphite is small, and it cannot store a large amount of sodium ions. When used as a negative electrode material for sodium-ion batteries, it is impossible to form a stable intercalation compound, which makes graphite unable to be used as a negative electrode material for sodium-ion batteries.

[0004] Compared with graphite, amorphous carbon has a wide range of raw materials and does not require graphitization in its preparation. It has great advantages in energy conservation, emission reduction and unit manufacturing cost, making it possible for large-scale application. In addition, amorphous carbon has a short-range ordered and long-range interlaced layered structure and a large interlayer spacing. + and Na + It can be easily embedded and de-embedded from all angles, which improves the diffusion coefficient of ions and thus achieves the effect of low-temperature rapid charging and discharging. In addition, there are a large number of micropores and defects in the structure of amorphous materials, which provide abundant active sites for ion storage. Its theoretical reversible capacity is much greater than the theoretical capacity of graphite, 372mAh / g. Therefore, amorphous carbon negative electrode materials are expected to be used in future energy storage battery applications.

[0005] Although amorphous carbon negative electrode materials have many advantages, there are still many problems in the application process, such as: (1) Due to the limitations of precursor structure and existing process technology, the reversible capacity of existing amorphous carbon products on the market is low, which affects the design and use of battery cells; (2) There are many defects and active sites on the surface of the material, the first coulomb efficiency is low, which reduces the energy density of the battery, and it is easy to react with the electrolyte at high temperature, resulting in rapid capacity decay; (3) The crystallinity of the material is generally small, which reduces the electronic conductivity and increases the polarization of the battery; (4) The abundant pores and functional groups on the surface of the material are prone to chemical adsorption, and the storage energy can adsorb small molecular impurities in the air environment, resulting in a sharp decrease in reversible capacity and cycle stability. Therefore, the promotion and application of amorphous carbon materials are limited.

[0006] Therefore, in order to improve and overcome the problems existing in the use of amorphous carbon as a negative electrode material and at the same time meet the commercial application needs of lithium-ion batteries and sodium-ion batteries, it is urgent to develop a new process technology with wide applicability and a new structure of amorphous carbon with high performance characteristics. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a modified porous amorphous carbon negative electrode material and a preparation method and application thereof. By processing the material, a composite material with a specific pore size distribution is obtained. Combined with the doping of specific elements, the material has high reversible mass specific capacity, high first coulomb efficiency, excellent conductivity and low-temperature and high-rate charge and discharge cycle retention characteristics. The surface is adsorbent and has good environmental tolerance stability. The problem of performance attenuation of amorphous carbon negative electrode materials after long-term placement in an air environment is effectively solved, filling the gap in the prior art.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] The technical purpose of the first aspect of the present invention is to provide a modified porous amorphous carbon negative electrode material, which has a core-shell structure, wherein the core is porous amorphous carbon doped with F elements, and the shell is a mixture of amorphous carbon and conductive carbon. The modified porous amorphous carbon negative electrode material has micropores, mesopores and macropores. Based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 5-40% of the total pore volume, the mesopores account for 15-70% of the total pore volume, and the macropores account for 10-50% of the total pore volume.

[0010] It should be understood by those skilled in the art that the above-mentioned "micropores" in this article refer to pores with a pore diameter less than 2nm, the "mesopores" refer to pores with a pore diameter of 2nm-50nm, and the "macropores" refer to pores with a pore diameter greater than 50nm. In the present invention, they particularly refer to pores greater than 50nm and not greater than 150nm.

[0011] Preferably, based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 5-30% of the total pore volume, the mesopores account for 30-70% of the total pore volume, and the macropores account for 15-40% of the total pore volume.

[0012] More preferably, based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 8-25% of the total pore volume, the mesopores account for 40-70% of the total pore volume, and the macropores account for 20-35% of the total pore volume.

[0013] Preferably, the total pore volume of the modified porous amorphous carbon negative electrode material is 0.03-1.0 cm 3 / g, for example 0.05cm 3 / g, 0.15cm 3 / g, 0.25cm 3 / g, 0.35cm 3 / g, 0.55cm 3 / g, 0.75cm 3 / g, 0.95cm 3 / g, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] Preferably, in the shell, the conductive carbon is embedded in the amorphous carbon, and the embedding means that the conductive carbon is partially or completely buried in the internal structure of the amorphous carbon, and the amorphous carbon forms a coating or anchoring on the conductive carbon.

[0015] Preferably, the conductive carbon is a particle with a length or width of 3-50 μm, such as 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 8-30 μm. The multiple conductive carbon particles contained in the shell act as "cables" for electron transmission within the material particles and between the particles, enhancing the electron transferability.

[0016] As a preferred technical solution, the core further contains doping elements, and the doping elements include at least F and O. As a more preferred technical solution, the core further includes at least one of S and N.

[0017] Further, as a preferred technical solution, based on the total weight of the negative electrode material, the total carbon content is 85-96%, such as 85%, 87%, 89%, 90%, 92%, 94% or 96%, the oxygen content is 2-10%, such as 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, and the fluorine content is 0.01-5.0%, such as 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3. 0%, 4.0% or 5.0%, etc., the nitrogen content is 0-5%, such as 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 4.0% or 5.0%, etc., the sulfur content is 0-6%, such as 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 4.0%, 5.0% or 6.0%, etc., the above are not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] The present invention provides a carbon negative electrode material with high capacity, high rate charge and discharge and high conductivity. The material has a core-shell three-dimensional hierarchical pore structure: (1) the microporous structure and abundant heteroelement modification sites in the porous core carbon (i.e., the inner core) provide active sites for energy storage reactions, which helps to improve the mass specific capacity of the material; the mesoporous and macroporous structures can serve as channels for rapid transmission of electrolyte ions, which is conducive to large current charge and discharge and improves rate performance; (2) the shell carbon (i.e., the outer shell) on the surface of the material has extremely high density and adhesion uniformity, which can make the material present physical adsorption inertia. In addition, the fluorine element doped into the core carbon can form abundant hydrophobic functional groups, which improves the storage stability of the material; (3) the shell carbon is inlaid with conductive carbon, which can reduce the electronic impedance of the carbon particle body and the contact internal resistance between particles, and improve the electronic conductivity of the material.

[0019] The multi-core carbon refers to a carbon skeleton having micropores, mesopores and macropores. In the present invention, the core carbon is the first main part of the amorphous carbon negative electrode material.

[0020] The shell carbon refers to the enhanced carbon coated on the surface of the porous core carbon, which has a dense structure and a pore-filling and pore-shrinking effect, that is, the open micropores in the core carbon are converted into closed micropores, the open mesopores are converted into micropores, and the open macropores are converted into mesopores. In the present invention, the shell carbon is the second main part of the amorphous carbon negative electrode material.

[0021] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0022] As a preferred technical solution of the present invention, the modified porous amorphous carbon negative electrode material has an irregular multi-angular appearance, a smooth and flat surface, and a core-shell structure at the microscopic level, wherein the core layer is porous and rich in fluorine-modified functional groups, and the shell layer has a densified structure. This special structure plays an adsorption inert role and can prevent impurity gases in the air from entering the material structure. Therefore, the performance of the material is almost not attenuated after being placed in an air environment.

[0023] Preferably, the modified porous amorphous carbon negative electrode material is a core-shell hierarchical structure, the inner core is core carbon, the outer shell is shell carbon, and the inner core has a three-dimensional porous structure, where the three-dimensional refers to a spatial stereoscopic structure, i.e., the micropores, mesopores, and macropores are connected and interconnected with each other.

[0024] As a preferred technical solution of the present invention, the mass of the inner core accounts for 94-99.8% of the total weight of the modified porous amorphous carbon negative electrode material, such as 94%, 95%, 96%, 97%, 98% or 99%, etc., preferably 98-99.4%. The amorphous carbon in the outer shell accounts for 0.1-5% of the total weight of the modified porous amorphous carbon negative electrode material, such as 0.5%, 1.5%, 2.5%, 3.5%, 4.5% or 5.0%, etc., preferably 0.5-1.9%; the conductive carbon accounts for 0.01-1% of the total weight of the modified porous amorphous carbon negative electrode material, such as 0.05%, 0.15%, 0.35%, 0.55%, 0.75% or 0.95%, etc., preferably 0.02-0.5%; the above are not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the thickness of the shell is 10-500nm, such as 25nm, 50nm, 75nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or 500nm, etc., preferably 300-450nm. Here, if the thickness of the shell carbon is too thick, the compaction density of the modified porous amorphous carbon negative electrode material will decrease, the proportion of active core carbon will decrease, and the energy density will decrease; if the thickness of the shell carbon is too thin, it will be difficult to coat evenly, and the core carbon will be exposed, which will not achieve the effect of reducing the interface impedance and the closed-cell micropore shaping.

[0026] Preferably, the pore size of the micropores in the material of the present invention is 0.2-2 nm, such as 0.2 nm, 0.4 nm, 0.6 nm, 0.8 nm, 1.0 nm, 1.5 nm or 2 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 0.5-1 nm. Too large a micropore size will increase the irreversible reaction active sites between the material and the electrolyte, resulting in a decrease in the first effect.

[0027] Preferably, the pore size of the mesopores in the material of the present invention is 2-30 nm, for example 3 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 5-15 nm.

[0028] Preferably, the pore size of the macropores in the material of the present invention is 50-120 nm, for example, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 110 nm or 120 nm, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 50-100 nm.

[0029] Preferably, the median particle size D50 of the modified porous amorphous carbon negative electrode material is 2.0-35.0 μm, for example, 2.0 μm, 5.0 μm, 10.0 μm, 15.0 μm, 20.0 μm, 25.0 μm, 30.0 μm or 35.0 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 5-15 μm.

[0030] Preferably, the specific surface area of ​​the modified porous amorphous carbon negative electrode material is 1.5-30m 2 / g, for example 1.5m 2 / g, 3.5m 2 / g, 5m 2 / g, 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g or 30m 2 / g, etc., but are not limited to the listed values, other values ​​not listed in the numerical range are also applicable, preferably 5-15m 2 / g.

[0031] Preferably, the interlayer spacing d002 of the modified porous amorphous carbon negative electrode material is 0.350-0.400 nm, for example, 0.350 nm, 0.355 nm, 0.360 nm, 0.365 nm, 0.370 nm, 0.375 nm, 0.380 nm, 0.385 nm, 0.390 nm, 0.395 nm or 0.400 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 0.37-0.39 nm;

[0032] Preferably, the Raman spectrum D peak (~1340cm -1) integrated area and G peak (~1590cm -1 )Integrated area ratio (I D / I G ) is 0.80-2.00, for example 0.80, 1.00, 1.20, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90 or 2.00, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1.00-1.50.

[0033] Preferably, the powder resistivity of the modified porous amorphous carbon negative electrode material is 0.3-2.0Ωmm, for example, 0.3Ωmm, 0.5Ωmm, 0.7Ωmm, 0.9Ωmm, 1.0Ωmm, 1.2Ωmm, 1.4Ωmm, 1.6Ωmm, 1.8Ωmm or 2.0Ωmm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 0.3-1.6Ωmm.

[0034] Preferably, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 60-100°, for example, 60°, 63°, 65°, 68°, 70°, 73°, 75°, 78°, 80°, 82°, 85°, 88°, 90°, 93°, 95°, 97° or 100°, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0035] The technical purpose of the second aspect of the present invention is to provide a method for preparing the modified porous amorphous carbon negative electrode material as described in the first aspect, comprising:

[0036] The carbon-rich precursor is crushed to obtain carbon powder particles, and the carbon powder particles are mixed with a modifier containing at least F element for doping and modification to obtain doped carbon;

[0037] The doped carbon is subjected to chemical etching to form pores to obtain porous core carbon;

[0038] The core carbon is compositely coated and carbonized with amorphous carbon and conductive carbon to form a "core-shell" structure, thereby obtaining the modified porous amorphous carbon negative electrode material.

[0039] In the preparation method provided by the present invention, an adsorption-resistant doped porous modified amorphous carbon negative electrode material is prepared by means of low-temperature carbon skeleton modification, medium-temperature chemical reaction etching and high-temperature coating sintering auxiliary processes. Specifically, under low-temperature stirring conditions, an atomic substitution reaction occurs between carbon powder particles of a certain size and the target element modifier, and the carbon powder particles are further cross-linked and stabilized to form doped carbon powder particles, and then gradually react with a chemical etchant under relatively high medium temperature and stirring conditions, and some skeleton carbon atoms are activated to break bonds to form small molecular gas substances to be discharged, and the doped carbon powder particles are gradually porous to form micropores, mesopores and macropores with a certain pore size distribution. The multi-level pore structure formed above is then filled or closed by carbon source deposition or pyrolysis under high temperature conditions, and some open pores are converted into closed pores and the pore size of the open pores is reduced, and at the same time, conductive carbon coating is used to obtain a three-dimensional modified porous amorphous carbon negative electrode material. Due to the presence of hydrophobic groups in the structure of the modified porous amorphous carbon material, it has the function of resisting environmental adsorption. In addition, the carbon coating on the surface layer of the core carbon powder particles and the synergistic introduction of conductive carbon can further improve the electrochemical interface, reduce defects and enhance the electrochemical efficiency.

[0040] As a preferred technical solution of the present invention, the median particle size of the carbon powder particles is 1.5-30μm, for example, 1.5μm, 3μm, 5μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, 22μm, 25μm, 28μm or 30μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 5-15μm; here, if the carbon powder particles are too small, the material activity is large, the subsequent process is prone to over-etching, resulting in more macropores, and large material ablation losses. At the same time, too many macroporous structures will consume a large amount of electrolyte and reduce the initial efficiency; if the carbon powder particles are too large, it will also lead to uneven subsequent amorphous carbon and conductive carbon coating, and even direct uncoated areas.

[0041] Preferably, the method for doping and modifying the carbon powder particles by mixing and reacting with a modifier containing at least the element F comprises: heating the mixture of the carbon powder particles and the modifier to react, thereby obtaining the doped carbon; if the aforementioned modifier is in gas phase, it is introduced in gas form; if it is in liquid phase or solid phase, it is first mixed evenly with the carbon powder particles and then put into a reaction device for heating. Preferably, the modifier also contains at least one of the elements S and N.

[0042] Preferably, the modifier is fluorine gas, and can also selectively react with at least one modifier selected from sulfur dioxide, sulfur trioxide, ammonia, urea, melamine, oxygen, and hydrogen peroxide. The carbon powder particles can react with different modifiers individually or in a mixed reaction, and there is no order of precedence when reacting individually. The concentration of the fluorine gas is 5-90%, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 10-30%; the concentration of sulfur dioxide is 5-90%, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 10- 50%; the sulfur trioxide concentration is 5-90%, for example 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 10-40%; the oxygen concentration is 20-90%, for example 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 30-50%.

[0043] Preferably, the fluorine content of the doped carbon is 0.01-8%, such as 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the oxygen content is 2-20%, such as 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18% or 20%, etc., but is not limited to the listed values, and other values ​​within the numerical range are also applicable. The values ​​not listed are also applicable; the nitrogen content is 0-7%, such as 0%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6% or 7%, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the sulfur content is 0-8%, such as 0%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. Here, if the fluorine content, sulfur content, nitrogen content and oxygen content are too large, too many structural defects will be generated, resulting in a decrease in the initial efficiency of the final material.

[0044] Preferably, the reaction temperature of the doping modification is 100-500°C, for example, 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the reaction time of the doping modification is 1-6 h, such as 1 h, 2 h, 3 h, 4 h, 5 h or 6 h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the doping modification is carried out in a reactor with stirring;

[0047] Preferably, the stirring rate of the stirring is 5-100r / min, for example 5r / min, 10r / min, 20r / min, 30r / min, 40r / min, 50r / min, 60r / min, 70r / min, 80r / min, 90r / min or 100r / min, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 30-50r / min.

[0048] As a preferred technical solution of the present invention, the chemical etching method for pore formation includes gas phase etching activation and / or metal compound etching activation. The preferred gas phase etching can achieve uniform and orderly activation on the particle surface and shallow surface layer, and the metal compound etching can achieve deep activation in the radial direction of the particles.

[0049] Preferably, the median particle size of the core carbon is 1.5-30 μm, such as 1.5 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, 28 μm or 30 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 3-15 μm;

[0050] Preferably, the pore size of the micropores of the core carbon is 0.2-2 nm, such as 0.2 nm, 0.4 nm, 0.6 nm, 0.8 nm, 1.0 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm or 2.0 nm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 0.5-1.5 nm;

[0051] Preferably, the pore size of the mesopores of the core carbon in step (2) is 2-40 nm, such as 2 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm or 40 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 5-20 nm;

[0052] Preferably, the pore size of the macropores of the core carbon in step (2) is 50-150 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm or 150 nm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 50-100 nm;

[0053] Preferably, the total pore volume of the core carbon is 0.05-2.0 cm 3 / g, for example 0.05cm 3 / g, 0.1cm 3 / g, 0.3cm 3 / g, 0.5cm 3 / g, 0.8cm 3 / g, 1.2cm 3 / g, 1.5cm 3 / g, 1.8cm 3 / g or 2.0cm 3 / g, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the specific surface area of ​​the core carbon is 1.5-50m 2 / g, for example 1.5m 2 / g, 3m 2 / g, 5m 2 / g, 8m 2 / g, 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g, 35m 2 / g, 40m 2 / g, 45m 2 / g or 50m 2 / g, etc., but are not limited to the listed values, other values ​​not listed in the numerical range are also applicable, preferably 5-25m 2 / g;

[0055] Preferably, the gas phase etching activation method comprises: heating the doped carbon in a carbon dioxide and / or water vapor atmosphere to react, thereby obtaining the core carbon;

[0056] Preferably, the concentration of the carbon dioxide is 1-100%, such as 1%, 3%, 5%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100%, etc., but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 5-50%, and the balance gas is an inert atmosphere selected from at least one of nitrogen, helium, neon, argon or xenon;

[0057] Preferably, the water vapor is introduced at a rate of 0.1-300 g / min, such as 0.1 g / min, 1 g / min, 5 g / min, 10 g / min, 20 g / min, 30 g / min, 40 g / min, 50 g / min, 100 g / min, 150 g / min, 200 g / min, 250 g / min or 300 g / min, etc., but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 1-50 g / min, and the water vapor is generated by a steam generator;

[0058] Preferably, the reaction temperature of the vapor phase etching activation is 400-1200° C., such as 400° C., 500° C., 600° C., 700° C., 800° C., 900° C., 1000° C., 1100° C. or 1200° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0059] Preferably, the reaction time of the vapor phase etching activation is 0.5-6h, such as 0.5h, 1h, 2h, 3h, 4h, 5h or 6h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0060] Preferably, the heating reaction is carried out in a stirred or rotatable reactor;

[0061] Preferably, the stirring or rotation rate is 5-100r / min, for example 5r / min, 10r / min, 20r / min, 30r / min, 40r / min, 50r / min, 60r / min, 70r / min, 80r / min, 90r / min or 100r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 10-50r / min.

[0062] Preferably, the method for etching and activating the metal compound comprises: mixing the doped carbon and at least one selected from sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, calcium carbonate, zinc carbonate, sodium bicarbonate, potassium bicarbonate, calcium bicarbonate, iron carbonate, zinc chloride, zinc oxide, zinc acetate, sodium acetate, potassium acetate or calcium acetate for heating reaction, and then washing with acid and water to obtain the core carbon after drying. The above preferred composite metal compound has a low decomposition temperature, and the nano-metal oxide generated after decomposition can react with the carbon matrix to etch at high temperature, playing a composite activation role of micropores and mesopores. At the same time, the metal element after the reaction promotes the rearrangement of the carbon skeleton and improves the graphitization degree of the organic complex pyrolytic carbon.

[0063] Preferably, the mass ratio of the metal compound to the doped carbon is (0.02-1):1, such as 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably (0.05-0.5):1;

[0064] Preferably, the mixing method is stirring mixing;

[0065] Preferably, the reaction temperature of the metal compound etching activation is 500-1400°C, such as 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C or 1400°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0066] Preferably, the reaction time of the metal compound etching activation is 1-6 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0067] Preferably, the pickling is to mix the product obtained after the reaction with an acid in a mass ratio of 1:(0.3-50), such as 1:0.3, 1:0.5, 1:1, 1:2, 1:5, 1:10, 1:20, 1:30, 1:40 or 1:50, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1:(1-20);

[0068] Preferably, the pickling is carried out by using one or a combination of at least two of hydrochloric acid, nitric acid and hydrofluoric acid;

[0069] Preferably, the concentration of the acid is 0.5-5 mol / L, such as 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L or 5.0 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0070] Preferably, the water washing is repeated several times until the pH of the filtrate meets 6-7;

[0071] Preferably, the drying method is heating drying or supercritical drying;

[0072] Preferably, the ash content of the core carbon is less than 5%.

[0073] As a preferred technical solution of the present invention, the method of composite coating of the core carbon with amorphous carbon and conductive carbon includes vapor deposition coating and / or liquid phase coating; the above coating process can achieve precise and uniform coating of the particle surface, and the thickness of the coating layer is easy to adjust.

[0074] Preferably, the vapor deposition coating method comprises: subjecting the core carbon to a high-temperature carbon deposition reaction under a carbon source gas to generate an amorphous carbon coating layer on the surface of the material, and then uniformly mixing the obtained product with a conductive carbon slurry under high-speed stirring, and sintering the product through high-temperature carbonization;

[0075] Preferably, the carbon source is selected from one or a combination of at least two of saturated hydrocarbons, aromatic hydrocarbons, alkenes, alkynes, alcohols, aldehydes, carboxylic acids and esters containing 1 to 8 carbon atoms, and more preferably one or a combination of at least two of methane, ethane, propane, butane, ethylene, propylene, butene, acetylene, methanol, ethanol, cyclohexane, cyclopentane, toluene, xylene and aniline;

[0076] Preferably, the reaction temperature of the carbon deposition reaction is 700-1300° C., for example, 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1150° C., 1200° C., 1250° C. or 1300° C., etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0077] Preferably, the carbon source introduction rate is 0.2-80 g / min, such as 0.2 g / min, 0.5 g / min, 1 g / min, 2 g / min, 5 g / min, 10 g / min, 15 g / min, 20 g / min, 30 g / min, 40 g / min, 50 g / min, 60 g / min, 70 g / min or 80 g / min, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 1-30 g / min;

[0078] Preferably, the deposition reaction is carried out in a reaction device with stirring or rotation;

[0079] Preferably, the liquid phase coating method comprises: uniformly mixing the core carbon with the liquid phase coating agent and the conductive carbon slurry under high-speed stirring, and then carbonizing and sintering at high temperature;

[0080] Preferably, the liquid coating agent is selected from one or a combination of at least two of liquid asphalt, aromatic tar, monosaccharide solution, polysaccharide solution, citric acid solution, phenolic resin solution, epoxy resin solution, polyacrylonitrile solution and polyvinyl pyrrolidone solution; the mass fraction of the solute in the above solution is 5-90%, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 10-50%;

[0081] Preferably, the mass ratio of core carbon, shell carbon (amorphous carbon) and conductive carbon in the "core-shell" structure is 100:0.1-5:0.01-1, for example, 100:0.1:0.01, 100:0.3:0.05, 100:0.5:0.1, 100:1:0.3, 100:2:0.5, 100:3:0.7, 100:4:0.9 or 100:5:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 100:0.5-3:0.02-0.5;

[0082] Preferably, the conductive carbon precursor is conductive carbon slurry;

[0083] Preferably, the conductive carbon slurry comprises conductive carbon, a dispersing aid and a solvent, and the composition ratio by weight percentage is 0.01-10% of conductive carbon, 0.03-3% of dispersing aid and 87-99.96% of solvent;

[0084] Preferably, the conductive carbon is selected from one or a combination of at least two of single-walled carbon nanotubes, multi-walled carbon nanotubes, nanocarbon fibers, graphene and carbon black;

[0085] Preferably, the length of the carbon nanotube is 3-50 μm, for example, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 5-20 μm; the diameter of the nano carbon fiber is 0.6-100 nm, and the length is 5-50 μm; the number of graphene layers is 1-50, for example, 1 layer (single layer), 2 layers, 3 layers, 5 layers, 7 layers, 9 layers, 10 layers, 15 layers, 20 layers, 25 layers, 30 layers, 35 layers, 40 layers, 45 layers or 50 layers, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 3-10 layers;

[0086] Preferably, the dispersing aid is selected from at least one of polycarboxylic acids, polycarboxylates, polyethylene glycols, polyfluoroolefins, polysilanes, polyacrylic acids and silane coupling agents, and is further preferably selected from one or a combination of at least two of carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinylidene fluoride (PVDF), ethylene glycol, ethylenediaminetetraacetic acid, sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, polyethylene glycol, polysorbate-20, polysorbate-80 and polyethylene oxide-polypropylene oxide-polyethylene oxide copolymer (PEO-PPO-PEO);

[0087] Preferably, the solvent is selected from at least one of alcohols, ketones, esters, aromatic hydrocarbons, alicyclic hydrocarbons and water, and more preferably one or a combination of at least two of water, ethanol, N-methylpyrrolidone, toluene and washing oil;

[0088] Preferably, the conductive carbon slurry is prepared by adding conductive carbon and a dispersing aid into a solvent and stirring the mixture until uniformly mixed;

[0089] Preferably, the carbonization is carried out under an inert atmosphere;

[0090] Preferably, the inert atmosphere includes any one of a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere or a xenon atmosphere, or a combination of at least two thereof;

[0091] Preferably, the carbonization temperature is 800-1500°C, for example, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C or 1500°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0092] Preferably, the carbonization time is 0.5-6h, such as 0.5h, 1h, 2h, 3h, 4h, 5h or 6h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0093] Preferably, the carbonization heating rate is 0.5-20°C / min, for example, 0.5°C / min, 1°C / min, 2°C / min, 4°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min or 20°C / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0094] Preferably, the carbonization reactor comprises any one or a combination of at least two of a vacuum furnace, a box furnace, a tube furnace, a roller kiln, a push plate kiln, a microwave oven or an infrared pyrolysis furnace;

[0095] Preferably, the carbonization further comprises: cooling to 20-50° C. after sintering;

[0096] As a preferred technical solution of the present invention, the method for preparing the carbon powder particles comprises: crushing a carbon-rich precursor, or preferably crushing it after low-temperature pretreatment under a suitable atmosphere, to obtain the carbon powder particles;

[0097] Preferably, the carbon-rich precursor is selected from any one or a combination of at least two of coke, coal, asphalt, resin and biomass;

[0098] Preferably, the coke comprises any one of coal coke, petroleum coke, pitch coke, mesophase carbon microbeads or charcoal, or a combination of at least two thereof; the volatile matter content of the coke is 0.01-15%, such as 0.01%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 3-10%;

[0099] Preferably, the coal type includes any one of anthracite, bituminous coal, sub-bituminous coal or lignite, or a combination of at least two of them; the volatile matter content of the coal type is 0.1-50%, such as 0.1%, 0.5%, 1%, 3%, 5%, 7%, 9%, 10%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also included. The numerical values ​​are also applicable, preferably 10-40%; the ash content of the coal is 0.001-10%, such as 0.001%, 0.005%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 0.001-5%;

[0100] Preferably, the asphalt comprises any one of coal tar asphalt, petroleum asphalt or shale asphalt, or a combination of at least two thereof; the softening point of the asphalt is 20-350°C, such as 20°C, 50°C, 80°C, 100°C, 150°C, 200°C, 250°C, 280°C, 300°C or 350°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 150-280°C;

[0101] Preferably, the resin comprises any one or a combination of at least two of phenolic resin, epoxy resin, phenolic epoxy resin, furfural resin, petroleum resin, coumarone resin or polyimide resin;

[0102] Preferably, the inert atmosphere includes any one of a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere or a xenon atmosphere, or a combination of at least two thereof;

[0103] Preferably, the biomass comprises any one or a combination of at least two of lignin, microcrystalline cellulose, starch, fruit shell, apricot shell, peach shell, coconut shell, peanut shell, rice husk, cotton husk, sawdust, bamboo fiber or straw;

[0104] Preferably, the temperature of the low temperature pretreatment is 200-700°C, for example, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0105] Preferably, the heating rate of the low-temperature pretreatment is 0.5-20°C / min, for example, 0.5°C / min, 1°C / min, 2°C / min, 4°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min or 20°C / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0106] Preferably, the low temperature pretreatment time is 1-8h, such as 1h, 2h, 3h, 4h, 5h, 6h, 7h or 8h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0107] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0108] In a third aspect, the present invention provides a use of the modified porous amorphous carbon negative electrode material as described in the first aspect, wherein the modified porous amorphous carbon negative electrode material is used in a sodium ion battery, a lithium ion battery, a potassium ion battery or a supercapacitor.

[0109] Compared with the prior art, the present invention has the following beneficial effects:

[0110] (1) The modified porous amorphous carbon negative electrode material provided by the present invention has a special three-dimensional porous structure, wherein: ① The mesopore and macropore structure provide a fast transmission channel for electrolyte ions, accelerate the diffusion of electrochemical reaction ions, and are conducive to high current charging and discharging. The sodium removal capacity retention rate can reach more than 90% after 5000 cycles at a current density of 5C / 5C, which is better than the level of existing amorphous carbon materials (5C / 5C 3000 weeks about 85%); ② The rich microporous structure and heteroelement modification sites not only improve the material's mass specific capacity, when used as the negative electrode of a sodium ion battery, its first sodium removal capacity can reach more than 340mAh / g, and the first coulombic efficiency can reach more than 90%; it can also reduce the adsorption of the material, and the powder contact angle of the material can be increased from 51° to 85°. The prepared modified porous amorphous carbon negative electrode material is placed in the air for 30 days, and the reversible capacity and the first coulombic efficiency remain almost unchanged, which is much better than the level of existing amorphous carbon materials (the capacity retention rate after 30 days is about 90%), and significantly improves the problem of attenuation of amorphous carbon materials placed in the air.

[0111] (2) The present invention first prepares carbon powder particles from a carbon-rich precursor, then performs element modification and chemical etching on the obtained carbon powder particles to obtain a porous core carbon, and then performs surface coating and conductive carbon composite treatment on the obtained core carbon, successfully realizing the design and preparation of a highly conductive three-dimensional porous core-shell structure amorphous carbon negative electrode material. The inner core of the material has a rich microporous structure and heteroelement modification sites, which can provide active sites for energy storage reactions and help improve the mass specific capacity of the material; at the same time, the shell carbon on the surface of the material has extremely high density and adhesion uniformity, and the shell carbon is embedded with conductive carbon, which can reduce the electronic impedance of the carbon particle body and the contact internal resistance between particles, and improve the electronic conductivity of the material. In addition, the fluorine functional group doped into the core carbon has the function of stabilizing the material and resisting adsorption, which improves the storage stability of the material in the natural environment.

[0112] (3) The preparation method provided by the present invention has a simple operation process, readily available raw materials and is environmentally friendly, with low preparation cost, and the morphology of the modified porous amorphous carbon negative electrode material obtained is controllable and easy to mass produce. It has high application value in the fields of energy storage, two-wheeled low-speed vehicles, hybrid vehicles, electric tools, etc., and can meet the requirements of high-performance lithium / sodium ion batteries for the charge and discharge performance of negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0113] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0114] Figure 1 This is a scanning electron microscope image (SEM) of the modified porous amorphous carbon negative electrode material prepared in Example 1;

[0115] Figure 2 X-ray diffraction pattern (XRD) of the modified porous amorphous carbon negative electrode material prepared in Example 1

[0116] Figure 3 Raman spectrum of the modified porous amorphous carbon negative electrode material prepared in Example 1

[0117] Figure 4 This is the nitrogen adsorption / desorption curve of the modified porous amorphous carbon negative electrode material prepared in Example 1;

[0118] Figure 5 The pore size distribution curve of the modified porous amorphous carbon negative electrode material prepared in Example 1;

[0119] Figure 6The first sodium ion charge and discharge curve of the modified porous amorphous carbon negative electrode material prepared in Example 1;

[0120] Figure 7 This is the sodium ion charge and discharge performance attenuation curve of the modified porous amorphous carbon negative electrode material prepared in Example 1 placed in an air environment. DETAILED DESCRIPTION

[0121] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0122] In the following examples, the structure and properties of the modified porous amorphous carbon negative electrode material were determined by the following method:

[0123] The surface morphology and particle size of the samples were observed using a JSM-7500F scanning electron microscope (JEOL).

[0124] The microcrystalline structure of the sample was tested using a Rigaku D / max 2550V X-ray diffractometer. The ray source was CuKα, the wavelength was 0.154056nm, the acquisition range was 2-80°, and the step length was 0.2°. Jade6.0 software was used to fit and analyze the diffraction data. Before the test, the instrument was calibrated with a Si standard sample to eliminate the instrument error. The interlayer spacing of the material was calculated using the Bragg equation: d 002 =λ / (2sinθ 002 ), where λ is the wavelength of the ray source, θ 002 is the Bragg angle of the (002) diffraction peak.

[0125] The sample structure was analyzed and tested using the InVia-Reflex Raman spectrometer from Renishaw, UK.

[0126] The specific surface area, pore volume and pore size distribution of the material were tested using an American Micromeritics ASAP 2460 fully automatic specific surface area and porosity analyzer.

[0127] Malvern laser particle size tester Mastersizer 3000 was used to test the particle size range of the material and the average particle size of the raw material particles.

[0128] The mass ratio of core carbon, shell carbon and conductive carbon in the negative electrode materials prepared in the embodiments and comparative examples is calculated according to the following principles: the weight of the core carbon is consistent with the feed amount of the carbon-rich precursor, the weight of the shell carbon is calculated based on the raw material feed amount and its pyrolysis residual carbon value, and the weight of the conductive carbon is consistent with the feed amount. The absolute weights of the three are normalized after being determined.

[0129] The content of each element in the negative electrode material was determined by X-ray fluorescence analysis (XRF).

[0130] The contact angle between the negative electrode material and water was measured using a contact angle meter.

[0131] The powder resistivity of the negative electrode material was measured by the four-electrode contact method at room temperature. The powder sample was loaded into a Teflon cylinder with an inner diameter of 16 mm, and then a pressure of 4 MPa was applied to the powder by two stainless steel pistons placed above and below the cylinder, and the current and voltage were recorded using a Keithley 2000.

[0132] Example 1

[0133] (1) Petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 8±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine are sequentially introduced for a reaction of 1h, followed by cooling to less than 50°C to obtain doped carbon.

[0134] (2) The doped carbon obtained in step (1) is further placed in a rotary kiln and heated to 600°C at a heating rate of 5°C / min, and then water vapor is introduced at a steam generation rate of 30g / min to perform an etching reaction for 2h, and then cooled to less than 50°C to obtain a core carbon.

[0135] (3) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.4:2.0:97.6 to obtain a conductive carbon slurry. The core carbon obtained in step (2), liquid asphalt with a coking value of 15%, and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred for 20 minutes at a speed of 600 rpm (linear speed greater than 3 m / s). The mixture is then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 hours. The mixture is then cooled to less than 50°C, demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0136] The above method was used to test the material prepared in this example:

[0137] Figure 1 This is a scanning electron microscope image of the modified porous amorphous carbon negative electrode material prepared in Example 1. From the image, it can be seen that the particle surface of the amorphous carbon negative electrode material is smooth and dense, presents an irregular multi-angular appearance, the particle size is uneven, the particle size distribution is wide, and the particle size is about 8μm.

[0138] Figure 2 This is the X-ray diffraction pattern (XRD) of the modified porous amorphous carbon negative electrode material prepared in Example 1. It can be seen from the figure that bun-shaped diffraction peaks appear near 2θ=23° and 44°, corresponding to the (002) and (100) crystal plane structures of carbon, respectively, indicating that the obtained hard carbons are all typical amorphous carbon structures with a low degree of graphitization and an interlayer spacing basically located near 0.375nm.

[0139] Figure 3 This is the Raman spectrum (Raman) of the modified porous amorphous carbon negative electrode material prepared in Example 1. It can be seen from the figure that the sample has a peak at 1340 cm -1 and 1590cm -1 There are two typical Raman absorption peaks on the left and right, corresponding to sp 3 The D peak (defects and amorphous structure) and sp peak formed by the vibration of hybrid carbon atoms 2 Carbon Atom E 2g The G peak (ordered carbon layer structure) formed by vibration, the area ratio of the D peak to the G peak (I D / I G ) is 1.7.

[0140] Figure 4 is the nitrogen adsorption curve of the modified porous amorphous carbon negative electrode material prepared in this example, Figure 4 It can be seen that the material exhibits type IV adsorption-desorption isotherm characteristics. Its adsorption isotherm has a large adsorption amount in the low pressure region (P / P0) <0.1, indicating that there are abundant microporous structures in the material, and there is also an increase in nitrogen adsorption between the relative pressure (P / P0) 0.6-0.99, indicating that there are a certain number of medium and large pore structures in the material.

[0141] Figure 5 is the pore size distribution curve of the modified porous amorphous carbon negative electrode material prepared in this embodiment, Figure 5 It can be seen that the pore size of the macropores in the material structure is 50-120 nm, the pore size of the mesopores is 5-50 nm, and the pore size of the micropores is 1-2 nm.

[0142] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.78% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.19% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.04% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 350nm, the pore size of the macropore is 50-120nm, the pore size of the mesopore is 5-50nm, and the pore size of the micropore is 1-2nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.083cm 3 / g, wherein the micropore volume accounts for 12% of the total pore volume, the mesopore volume accounts for 63% of the total pore volume, and the macropore volume accounts for 25% of the total pore volume; the median particle size (D v 50) is 8.5 μm, and the specific surface area is 4.7 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 72° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 92.0%, the oxygen content is 4.1%, the fluorine content is 2.1%, the nitrogen content is 1.3%, and the sulfur content is 0.5%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 0.3Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 0. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 1.7.

[0143] Example 2

[0144] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0145] (1) Petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 5±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine are sequentially introduced for a reaction of 1h, followed by cooling to less than 50°C to obtain doped carbon.

[0146] (2) The doped carbon obtained in step (1) is mixed with fine particle KOH in a mass ratio of 100:5 in a high-speed mixer for 2 hours, and then placed in a rotary furnace and heated to 800°C at a heating rate of 5°C / min for etching reaction for 2 hours, cooled to less than 50°C, and then immediately placed in a reaction tank with 1 mol / L hydrochloric acid in a mass ratio of 1:1 (hydrochloric acid) and stirred at 60°C for reaction for 6 hours, and then filtered and washed until the pH of the filtrate reaches 7, and the filter cake is dried to obtain the core carbon.

[0147] (3) Multi-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.6:2.0:97.4 to obtain a conductive carbon slurry. The core carbon obtained in step (2) and liquid asphalt with a coking value of 15% and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred for 20 minutes at a speed of 600 rpm (linear speed greater than 3 m / s). The mixture is then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 hours. The mixture is then cooled to less than 50°C, demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0148] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0149] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.76% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.19% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.05% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 340nm, the pore size of the macropore is 50-90nm, the pore size of the mesopore is 3-35nm, and the pore size of the micropore is 0.5-1.2nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.128cm 3 / g, wherein the micropore volume accounts for 18% of the total pore volume, the mesopore volume accounts for 61% of the total pore volume, and the macropore volume accounts for 21% of the total pore volume; the median particle size (D v 50) is 5.3 μm, and the specific surface area is 5.5 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 77° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 91.4%, the oxygen content is 5.0%, the fluorine content is 1.8%, the nitrogen content is 1.2%, and the sulfur content is 0.6%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 0.8Ωmm, and the interlayer spacing parameter d of the modified porous amorphous carbon negative electrode material is 0.002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 1.8.

[0150] Example 3

[0151] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0152] (1) The corn starch is air flow crushed and the Dv50 is controlled at 10±0.5 μm. Then, it is placed in a rotary kiln under an excess air atmosphere and heated to 200°C at a speed of 5 r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 12 h. Then, the atmosphere is switched to a nitrogen atmosphere and the temperature is raised to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine are sequentially introduced for a reaction of 1 h, and then cooled to less than 50°C to obtain doped carbon.

[0153] (2) The doped carbon obtained in step (1) is further placed in a rotary furnace and heated to 1000° C. at a heating rate of 5° C. / min, and then 20% concentration CO2 is introduced for etching reaction for 2 hours, and then cooled to less than 50° C. to obtain core carbon.

[0154] (3) Nano carbon black, dispersant PVDF, and solvent NMP are mixed uniformly in a mass ratio of 1:2.0:97 to obtain a conductive carbon slurry. The core carbon obtained in step (2) and a phenolic resin solution with a coking value of 25% and the conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:6:8 and stirred for 20 minutes at a speed of 600 rpm (linear speed greater than 3 m / s). The mixture is then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 hours. The mixture is then cooled to less than 50°C, demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0155] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0156] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.43% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.48% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.10% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 400nm, the pore size of the macropore is 60-80nm, the pore size of the mesopore is 2-23nm, and the pore size of the micropore is 0.2-1.8nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.192cm3 / g, wherein the micropore volume accounts for 21% of the total pore volume, the mesopore volume accounts for 47% of the total pore volume, and the macropore volume accounts for 32% of the total pore volume; the median particle size (D v 50) is 10.2 μm, and the specific surface area is 5.9 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 75° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 89.9%, the oxygen content is 7.4%, the fluorine content is 1.6%, the nitrogen content is 0.8%, and the sulfur content is 0.3%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 1.2Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 1.2Ωmm. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 2.0.

[0157] Example 4

[0158] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0159] (1) Clean coal with a volatile content of 20-22% is crushed by air flow and the Dv50 is controlled at 8±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 15% sulfur dioxide, 15% ammonia, and 15% fluorine are sequentially introduced for a reaction of 1h, followed by cooling to less than 50°C to obtain doped carbon.

[0160] (2) The doped carbon obtained in step (1) is further placed in a rotary kiln and heated to 600°C at a heating rate of 5°C / min, and then water vapor is introduced at a steam generation rate of 30g / min for etching reaction for 2h to obtain core carbon. The atmosphere is then switched to nitrogen, and the temperature is increased to 850°C at a heating rate of 2°C / min. Then, 25g / min of methane is introduced for carbon deposition coating for 1h, and the carbon is cooled to less than 50°C to obtain coated core carbon.

[0161] (3) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.4:2.0:97.6 to obtain a conductive carbon slurry. The coated core carbon obtained in step (2) and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8 and stirred at a speed of 600 rpm (linear speed greater than 3 m / s) for 20 min. The mixture is then placed in a box furnace and heated to 1250° C. at a heating rate of 5° C. / min for carbonization for 4 h. The mixture is then cooled to less than 50° C., demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0162] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0163] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.10% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.72% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.18% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 450nm, the pore size of the macropore is 60-100nm, the pore size of the mesopore is 5-38nm, and the pore size of the micropore is 0.8-1.7nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.067cm 3 / g, wherein the micropore volume accounts for 9% of the total pore volume, the mesopore volume accounts for 65% of the total pore volume, and the macropore volume accounts for 26% of the total pore volume; the median particle size (D v 50) is 7.8 μm, and the specific surface area is 3.8 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 83° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 93.1%, the oxygen content is 4.6%, the fluorine content is 1.1%, the nitrogen content is 1.0%, and the sulfur content is 0.2%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 0.5Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 0. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 1.4.

[0164] Example 5

[0165] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0166] (1) Clean coal with a volatile content of 20-22% is crushed by air flow and the Dv50 is controlled at 8±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and the temperature is raised to 500°C at a heating rate of 5°C / min. A 15% concentration of fluorine gas is introduced for a modification reaction for 2h, and then cooled to less than 50°C to obtain doped carbon.

[0167] (2) The doped carbon obtained in step (1) is further placed in a rotary furnace and heated to 1000° C. at a heating rate of 5° C. / min, and then 20% concentration CO2 is introduced for etching reaction for 2 hours, and then cooled to less than 50° C. to obtain core carbon.

[0168] (3) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.4:2.0:97.6 to obtain a conductive carbon slurry. The core carbon obtained in step (2), liquid asphalt with a coking value of 15%, and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred for 20 minutes at a speed of 600 rpm (linear speed greater than 3 m / s). The mixture is then placed in a box furnace and heated to 1250°C at a heating rate of 5°C / min for carbonization for 4 hours. The mixture is then cooled to less than 50°C, demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0169] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0170] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.78% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.18% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.04% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 350nm, the pore size of the macropore is 50-70nm, the pore size of the mesopore is 3-28nm, and the pore size of the micropore is 0.1-1.7nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.236cm 3 / g, wherein the micropore volume accounts for 23% of the total pore volume, the mesopore volume accounts for 49% of the total pore volume, and the macropore volume accounts for 28% of the total pore volume; the median particle size (D v 50) is 8.3 μm, and the specific surface area is 7.1 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 85° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 95.2%, the oxygen content is 3.6%, the fluorine content is 1.2%, the powder resistivity of the modified porous amorphous carbon negative electrode material is 0.7Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 0. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 1.5.

[0171] Example 6

[0172] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0173] (1) Coconut shells were placed in a rotary kiln under a nitrogen atmosphere and heated to 450°C at a speed of 5 r / min and a heating rate of 5°C / min for constant temperature pre-carbonization for 2 h. The atmosphere was then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine were introduced in sequence for reaction for 1 h, followed by cooling to less than 50°C, pulverizing with air flow and controlling Dv50 at 8±0.5 μm to obtain doped carbon.

[0174] (2) The doped carbon obtained in step (1) is further placed in a rotary kiln and heated to 600°C at a heating rate of 5°C / min, and then water vapor is introduced at a steam generation rate of 30g / min for etching reaction for 2h to obtain core carbon. The atmosphere is then switched to nitrogen, and the temperature is increased to 850°C at a heating rate of 2°C / min. Then, 25g / min of methane is introduced for carbon deposition coating for 1h, and the carbon is cooled to less than 50°C to obtain coated core carbon.

[0175] (3) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.4:

[0176] 2.0:97.6 are mixed evenly to obtain a conductive carbon slurry, the coated core carbon obtained in step (2) and the aforementioned conductive carbon slurry are put into a high-speed mixer at a mass ratio of 100:8, stirred at a speed of 600 rpm (linear speed greater than 3 m / s) for 20 min, then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 h, then cooled to less than 50°C, demagnetized and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0177] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0178] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.10% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.72% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.18% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 450nm, the pore size of the macropore is 50-90nm, the pore size of the mesopore is 3-40nm, and the pore size of the micropore is 1-2nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.098cm 3 / g, wherein the micropore volume accounts for 10% of the total pore volume, the mesopore volume accounts for 60% of the total pore volume, and the macropore volume accounts for 30% of the total pore volume; the median particle size (D v 50) is 8.5 μm, and the specific surface area is 4.9 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 74° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 92.0%, the oxygen content is 6.1%, the fluorine content is 0.9%, the nitrogen content is 0.8%, and the sulfur content is 0.2%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 1.5Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 1.5Ωmm. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 1.9.

[0179] Example 7

[0180] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0181] (1) The coconut shell was placed in a rotary kiln under a nitrogen atmosphere and heated to 450°C at a speed of 5 r / min and a heating rate of 5°C / min for constant temperature pre-carbonization for 2 h, then heated to 500°C at a heating rate of 2°C / min, and then introduced into a 10% concentration of fluorine gas for modification reaction for 2 h, and then cooled to less than 50°C, and pulverized by air flow and controlled Dv50 at 8±0.5 μm to obtain doped carbon

[0182] (2) The doped carbon obtained in step (1) is mixed with fine particle KOH in a mass ratio of 100:5 in a high-speed mixer for 2 hours, and then placed in a rotary furnace and heated to 800°C at a heating rate of 5°C / min for etching reaction for 2 hours, cooled to less than 50°C, and then immediately placed in a reaction tank with 1 mol / L hydrochloric acid in a mass ratio of 1:1 (hydrochloric acid) and stirred at 60°C for reaction for 6 hours, and then filtered and washed until the pH of the filtrate reaches 7, and the filter cake is dried to obtain the core carbon.

[0183] (3) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are mixed in a mass ratio of 0.4:

[0184] 2.0:97.6 is mixed evenly to obtain a conductive carbon slurry, the core carbon obtained in step (2), the phenolic resin solution with a coking value of 25% and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:6:8 and stirred at a speed of 600 rpm (linear speed greater than 3 m / s) for 20 min, then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 h, then cooled to less than 50°C, demagnetized and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0185] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0186] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.49% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.48% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.03% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 390nm, the pore size of the macropore is 50-80nm, the pore size of the mesopore is 2-30nm, and the pore size of the micropore is 0.5-1.5nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.185cm 3 / g, wherein the micropore volume accounts for 21% of the total pore volume, the mesopore volume accounts for 56% of the total pore volume, and the macropore volume accounts for 23% of the total pore volume; the median particle size (D v 50) is 8.8 μm, and the specific surface area is 5.6 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 78° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 93.1%, the oxygen content is 6.0%, the fluorine content is 0.9%, the powder resistivity of the modified porous amorphous carbon negative electrode material is 1.9Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 1.9Ωmm.002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 2.0.

[0187] Example 8

[0188] In this embodiment, the modified porous amorphous carbon negative electrode material is prepared according to the following method:

[0189] (1) A commercially available phenolic resin was cured at 120°C for 2 h, and after being roughly broken, it was placed in a rotary kiln under a nitrogen atmosphere and heated to 500°C at a speed of 5 r / min and a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine were introduced in sequence for reaction for 1 h, followed by cooling to less than 50°C, and pulverized with air flow to obtain doped carbon with Dv50 controlled at 10±0.5 μm.

[0190] (2) The doped carbon obtained in step (1) is further placed in a rotary kiln and heated to 600°C at a heating rate of 5°C / min, and then water vapor is introduced at a steam generation rate of 30g / min to perform an etching reaction for 2h, and then cooled to less than 50°C to obtain a core carbon.

[0191] (3) The few-layer graphene, dispersant PVDF, and solvent NMP are uniformly mixed in a mass ratio of 0.6:2.0:97.4 to obtain a conductive carbon slurry, and the core carbon obtained in step (2) and the liquid asphalt with a coking value of 15% and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred at a speed of 600 rpm (linear speed greater than 3 m / s) for 20 min. Then, the mixture is placed in a box furnace and heated to 1400°C at a heating rate of 5°C / min and carbonized for 4 h. Then, the mixture is cooled to less than 50°C, demagnetized, and sieved to obtain the modified porous amorphous carbon negative electrode material with a core-shell structure.

[0192] The modified porous amorphous carbon negative electrode material obtained in this example was subjected to structural testing using the method of Example 1:

[0193] In the modified porous amorphous carbon negative electrode material prepared in this embodiment, the mass of the core carbon accounts for 98.76% of the total mass of the modified porous amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.19% of the total mass of the modified porous amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.06% of the total mass of the modified porous amorphous carbon negative electrode material. The thickness of the shell carbon is 340nm, the pore size of the macropore is 50-100nm, the pore size of the mesopore is 5-40nm, and the pore size of the micropore is 0.8-2nm; the total pore volume of the modified porous amorphous carbon negative electrode material is 0.215cm 3 / g, wherein the micropore volume accounts for 16% of the total pore volume, the mesopore volume accounts for 51% of the total pore volume, and the macropore volume accounts for 33% of the total pore volume; the median particle size (D v 50) is 9.7 μm, and the specific surface area is 6.8 m 2 / g, the powder contact angle of the modified porous amorphous carbon negative electrode material with water is 72° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the modified porous amorphous carbon negative electrode material is 91.2%, the oxygen content is 7.2%, the fluorine content is 0.7%, the nitrogen content is 0.6%, and the sulfur content is 0.3%. The powder resistivity of the modified porous amorphous carbon negative electrode material is 1.1Ωmm, and the interlayer parameter d of the modified porous amorphous carbon negative electrode material is 1.1Ωmm. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the modified porous amorphous carbon negative electrode material (I D / I G ) is 2.0.

[0194] Comparative Example 1

[0195] The specific preparation method of this comparative example refers to Example 1, except that no activation operation is performed.

[0196] (1) Petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 8±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine are sequentially introduced for a reaction of 1h, followed by cooling to less than 50°C to obtain doped carbon.

[0197] (2) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are uniformly mixed in a mass ratio of 0.4:2.0:97.6 to obtain a conductive carbon slurry. The doped carbon obtained in step (1) and liquid asphalt with a coking value of 15% and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred for 20 minutes at a speed of 600 rpm (linear speed greater than 3 m / s). The mixture is then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 hours. The mixture is then cooled to less than 50°C and demagnetized and sieved to obtain the comparative amorphous carbon negative electrode material.

[0198] The structure of the comparative amorphous carbon negative electrode material obtained in this comparative example was tested using the method of Example 1:

[0199] In the comparative amorphous carbon negative electrode material prepared in this comparative example, the mass of the doped carbon accounts for 98.78% of the total mass of the comparative amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.19% of the total mass of the comparative amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.04% of the total mass of the comparative amorphous carbon negative electrode material. The thickness of the shell carbon is 350nm, the pore size of the macropore is 50-70nm, the pore size of the mesopore is 3-25nm, and there is no microporous structure; the total pore volume of the comparative amorphous carbon negative electrode material is 0.010cm 3 / g, of which the mesopore volume accounts for 47% of the total pore volume, and the macropore volume accounts for 53% of the total pore volume; the median particle size (D v 50) is 8.5 μm, and the specific surface area is 2.0 m 2 / g, the powder contact angle of the comparative amorphous carbon negative electrode material with water is 71° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the comparative amorphous carbon negative electrode material is 92.6%, the oxygen content is 4.0%, the fluorine content is 1.8%, the nitrogen content is 1.2%, and the sulfur content is 0.4%. The powder resistivity of the comparative amorphous carbon negative electrode material is 0.3Ωmm, and the interlayer spacing parameter d of the comparative amorphous carbon negative electrode material is 0. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the amorphous carbon negative electrode material (I D / I G ) is 1.2.

[0200] Comparative Example 2

[0201] The specific preparation method of this comparative example refers to that of Example 1, except that no activation and coating operations are performed.

[0202] (1) Petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 8±0.5μm. It is then placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. The atmosphere is then switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide, 10% ammonia, and 10% fluorine are sequentially introduced for a reaction of 1h, followed by cooling to less than 50°C to obtain doped carbon.

[0203] (2) The doped carbon obtained in step (1) is placed in a box furnace and heated to 1300° C. at a heating rate of 5° C. / min and carbonized for 4 hours, and then cooled to less than 50° C. and demagnetized and sieved to obtain the comparative amorphous carbon negative electrode material.

[0204] The structure of the comparative amorphous carbon negative electrode material obtained in this comparative example was tested using the method of Example 1:

[0205] The comparative amorphous carbon negative electrode material prepared in this comparative example has no core-shell structure, the macropore diameter of the comparative amorphous carbon negative electrode material is 50-80nm, the mesopore diameter is 15-45nm, and there is no microporous structure; the total pore volume of the comparative amorphous carbon negative electrode material is 0.012cm 3 / g, of which the mesopore volume accounts for 43% of the total pore volume, and the macropore volume accounts for 57% of the total pore volume; the median particle size (D v 50) is 8.1 μm, and the specific surface area is 2.6 m 2 / g, the powder contact angle of the comparative amorphous carbon negative electrode material with water is 73° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the comparative amorphous carbon negative electrode material is 93.8%, the oxygen content is 2.7%, the fluorine content is 2.1%, the nitrogen content is 0.9%, and the sulfur content is 0.5%. The powder resistivity of the comparative amorphous carbon negative electrode material is 6.3Ωmm, and the interlayer spacing parameter d of the comparative amorphous carbon negative electrode material is 1.3Ωmm. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the amorphous carbon negative electrode material (I D / I G ) is 1.3.

[0206] Comparative Example 3

[0207] The specific preparation method of this comparative example refers to that of Example 1, except that no F doping modification operation is performed.

[0208] (1) Petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 8±0.5μm. Then, it is placed in a rotary kiln under an excess air atmosphere and heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h. Then, the atmosphere is switched to a nitrogen atmosphere and the temperature is raised to 500°C at a heating rate of 5°C / min. Then, 10% sulfur dioxide and 10% ammonia are sequentially introduced for a reaction for 1h and 1h, and then cooled to less than 50°C. Then, the temperature is raised to 600°C at a heating rate of 5°C / min, and then water vapor is introduced at a steam generation rate of 30g / min for an etching reaction for 2h, and then cooled to less than 50°C to obtain a core carbon.

[0209] (2) Single-walled carbon nanotubes with an average length of 10 μm, dispersant PVDF, and solvent NMP are uniformly mixed in a mass ratio of 0.4:2.0:97.6 to obtain a conductive carbon slurry; the core carbon obtained in step (1), liquid asphalt with a coking value of 15%, and the aforementioned conductive carbon slurry are put into a high-speed mixer in a mass ratio of 100:8:10 and stirred at a speed of 600 rpm (linear speed greater than 3 m / s) for 20 min, then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min and carbonized for 4 h, then cooled to less than 50°C, demagnetized and sieved to obtain the comparative amorphous carbon negative electrode material.

[0210] The structure of the comparative amorphous carbon negative electrode material obtained in this comparative example was tested using the method of Example 1:

[0211] In the comparative amorphous carbon negative electrode material prepared in this comparative example, the mass of the core carbon accounts for 98.78% of the total mass of the comparative amorphous carbon negative electrode material, the mass of the shell carbon accounts for 1.19% of the total mass of the comparative amorphous carbon negative electrode material, and the mass of the conductive carbon accounts for 0.04% of the total mass of the comparative amorphous carbon negative electrode material. The thickness of the shell carbon is 350nm, the pore size of the macropore is 50-70nm, the pore size of the mesopore is 5-30nm, and the pore size of the micropore is 1.5-2nm; the total pore volume of the comparative amorphous carbon negative electrode material is 0.063cm 3 / g, of which the micropore volume accounts for 6% of the total pore volume, the mesopore volume accounts for 71% of the total pore volume, and the macropore volume accounts for 23% of the total pore volume; the median particle size (D v 50) is 7.8 μm, and the specific surface area is 4.2 m 2 / g, the powder contact angle of the comparative amorphous carbon negative electrode material with water is 53° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the comparative amorphous carbon negative electrode material is 93.0%, the oxygen content is 5.8%, the nitrogen content is 0.8%, the sulfur content is 0.4%, the powder resistivity of the comparative amorphous carbon negative electrode material is 0.3Ωmm, and the interlayer spacing parameter d of the comparative amorphous carbon negative electrode material is 0. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the comparative amorphous carbon negative electrode material (I D / I G ) is 1.6.

[0212] Comparative Example 4

[0213] The specific preparation method of this comparative example refers to that of Example 1, except that no doping modification, activation and coating operations are performed.

[0214] The petroleum asphalt with a softening point of 250°C is crushed by air flow and Dv50 is controlled at 8±0.5μm, then placed in a rotary kiln under an excess air atmosphere, heated to 230°C at a speed of 5r / min and a heating rate of 2°C / min for a constant temperature cross-linking reaction for 6h, then the atmosphere is switched to a nitrogen atmosphere and heated to 500°C at a heating rate of 5°C / min and then reacted at a constant temperature for 2h, cooled to less than 50°C and discharged, then placed in a box furnace and heated to 1300°C at a heating rate of 5°C / min for carbonization for 4h, then cooled to less than 50°C, demagnetized and sieved to obtain the comparative amorphous carbon negative electrode material

[0215] The structure of the comparative amorphous carbon negative electrode material obtained in this comparative example was tested using the method of Example 1:

[0216] The comparative amorphous carbon negative electrode material prepared in this comparative example has no core-shell structure, the macropore diameter of the comparative amorphous carbon negative electrode material is 80-100nm, the mesopore diameter is 20-45nm, and there is no microporous structure; the total pore volume of the comparative amorphous carbon negative electrode material is 0.096cm 3 / g, of which the mesopore volume accounts for 18% of the total pore volume, and the macropore volume accounts for 82% of the total pore volume; the median particle size (D v 50) is 8.3 μm, and the specific surface area is 4.9 m 2 / g, the powder contact angle of the comparative amorphous carbon negative electrode material with water is 51° (the powder contact angle between the amorphous carbon negative electrode material and cyclohexane is taken as the 0° baseline), the total carbon content of the comparative amorphous carbon negative electrode material is 94.0%, the oxygen content is 6.0%, the powder resistivity of the comparative amorphous carbon negative electrode material is 5.7Ωmm, and the interlayer spacing parameter d of the comparative amorphous carbon negative electrode material is 1.3Ωmm. 002 The integrated area ratio of the Raman spectrum D peak to the G peak of the comparative amorphous carbon negative electrode material (I D / I G ) is 1.1.

[0217] Application Examples

[0218] In the application examples, the performance of the above materials as battery negative electrode materials was tested:

[0219] The amorphous carbon negative electrode material prepared in each embodiment and comparative example was tested for the first specific capacity, first coulomb efficiency and cycle performance by a half-cell test method. The half-cell test method is as follows: the amorphous carbon negative electrode material, conductive carbon black, CMC, and SBR are mixed evenly in a mass ratio of 94.8:1.5:1.2:2.5, applied on a copper foil, and the coated electrode is placed in a vacuum drying oven at a temperature of 110°C for vacuum drying for 4 hours for standby use. Then, 1mol / L NaClO4 / EC+PC (v / v=1:1) is used as the electrolyte, and a glass fiber diaphragm and a metal sodium sheet are used as the counter electrode in an argon-filled German Mikaelona glove box to assemble a 2430-type button cell, charge with a current of 0.1C, discharge with a current of 0.1C, and test the first reversible capacity and the first coulomb efficiency on the blue battery test system. Furthermore, the negative electrode materials of each embodiment and comparative example were sampled and placed in the air for 30 days, and then the first reversible capacity and the first coulombic efficiency after 30 days were tested according to the above method.

[0220] The battery was charged at 5C and discharged at 5C, and the capacity retention rate was tested after 5000 cycles.

[0221] The above test results are shown in Table 1.

[0222] Table 1

[0223]

[0224] Figure 6 The first sodium ion charge and discharge curve of the modified porous amorphous carbon negative electrode material prepared in Example 1. It can be seen from the figure that the sodium insertion and deinsertion capacity of the modified porous amorphous carbon negative electrode material is 345 mAh / g and 381 mAh / g respectively;

[0225] Figure 7 The sodium ion charge and discharge performance attenuation curve of the modified porous amorphous carbon negative electrode material prepared in Example 1 placed in an air environment. It can be seen from the figure that after the modified porous amorphous carbon negative electrode material is placed for 30 days, its reversible sodium removal capacity is still 344mAh / g, and the first coulombic efficiency is 90.2%, which has excellent anti-adsorption properties.

[0226] Based on the above examples and comparative examples, it can be seen that Examples 1-8 first prepare carbon powder particles from a variety of carbon-rich precursors, then perform element modification and chemical etching on the obtained carbon powder particles to obtain porous core carbon, and then perform surface coating and conductive carbon composite treatment on the obtained core carbon to prepare a highly conductive three-dimensional porous core-shell structure amorphous carbon negative electrode material. The modified porous amorphous carbon negative electrode material prepared in Examples 1-8 exhibits excellent electrochemical properties in terms of first reversible capacity and high-rate long-cycle capacity retention rate, and the material surface is dense and has a rich fluorine-containing hydrophobic structure, which prevents moisture and other impurity gases in the air from entering the material structure. Therefore, after the material is placed in the air, the capacity and first effect are almost not attenuated.

[0227] In Comparative Example 1, the doped carbon was not subsequently etched to form pores, and the resulting material did not form abundant sodium storage holes and sites, and the reversible capacity was relatively low.

[0228] In Comparative Example 2, the doped carbon was not subsequently etched to form pores and surface coated, and the resulting material did not form abundant sodium storage holes and sites, and the exposed doping defects on the surface of the material increased, resulting in low reversible capacity and first coulombic efficiency.

[0229] In Comparative Example 3, the initial carbon powder particles were not modified by hydrophobic doping, and the resulting material had no adsorption inertness. After being placed in the air for 30 days, it adsorbed impurity gases in the air. These impurity gases formed chemical bonds with the carbon layer crystallites and the inner walls of the pores, occupying the existing active sites and increasing the irreversible active sites at the same time, resulting in a decrease in the reversible capacity and the first coulombic efficiency after air storage, and a deterioration in the air storage stability.

[0230] In Comparative Example 4, the initial carbon powder particles were not doped and modified, and subsequent etching and pore formation and surface coating were not performed, so a porous core-shell structure with performance enhancement and protection was not formed. Therefore, the initial reversible capacity and first coulombic efficiency of the material were low, and the material did not have a hydrophobic and anti-adsorption structure, and had poor air storage properties. After being placed in the air for 30 days, the reversible capacity and first coulombic efficiency were significantly reduced.

[0231] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A modified porous amorphous carbon negative electrode material, It is characterized in that It has a core-shell structure, wherein the core is porous amorphous carbon doped with F elements, and the shell is a mixture of amorphous carbon and conductive carbon. The modified porous amorphous carbon negative electrode material has micropores, mesopores and macropores. Based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 5-40% of the total pore volume, the mesopores account for 15-70% of the total pore volume, and the macropores account for 10-50% of the total pore volume. Preferably, based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 5-30% of the total pore volume, the mesopores account for 30-70% of the total pore volume, and the macropores account for 15-40% of the total pore volume. More preferably, based on the total pore volume of the modified porous amorphous carbon negative electrode material, the micropores account for 8-25% of the total pore volume, the mesopores account for 40-70% of the total pore volume, and the macropores account for 20-35% of the total pore volume.

2. The modified porous amorphous carbon negative electrode material according to claim 1, It is characterized in that The mass of the inner core accounts for 94-99.8% of the total weight of the modified porous amorphous carbon negative electrode material, preferably 98-99.5%; the amorphous carbon in the outer shell accounts for 0.1-5% of the total weight of the modified porous amorphous carbon negative electrode material, preferably 0.5-3%; the conductive carbon in the outer shell accounts for 0.01-1% of the total weight of the modified porous amorphous carbon negative electrode material, preferably 0.02-0.5%; The thickness of the shell is 10-500nm; The length or width of the conductive carbon is 3-50 μm, preferably 8-30 μm; The pore size of the micropores is greater than 0.2 nm and less than 2 nm, preferably 0.5-1 nm; the pore size of the mesopores is 2-30 nm, preferably 5-15 nm; the pore size of the macropores is greater than 50 nm and not greater than 120 nm, preferably greater than 50 nm and not greater than 100 nm; The total pore volume of the modified porous amorphous carbon negative electrode material is 0.03-1.0 cm3 / g; The modified porous amorphous carbon negative electrode material has an irregular multi-angular particle morphology and a smooth surface. The median particle size D50 of the modified porous amorphous carbon negative electrode material is 2.0-35.0 μm, preferably 5.0-15.0 μm; The specific surface area of ​​the modified porous amorphous carbon negative electrode material is 1.5-30m 2 / g, preferably 5-15m 2 / g; The interlayer spacing d of the modified porous amorphous carbon negative electrode material 002 0.350-0.400nm, preferably 0.370-0.390nm; The Raman spectrum D peak (~1340cm -1 ) integrated area and G peak (~1590cm -1 ) The integrated area ratio is 0.80-2.00, preferably 1.00-1.50; The powder resistivity of the modified porous amorphous carbon negative electrode material is 0.3-2.0Ωmm, preferably 0.3-1.6Ωmm; The powder contact angle of the modified porous amorphous carbon negative electrode material with water is 60-100°.

3. The modified porous amorphous carbon negative electrode material according to claim 1, It is characterized in that Based on the total weight of the negative electrode material, the total carbon content is 85-96%, the oxygen content is 2-10%, the nitrogen content is 0-5.0%, the fluorine content is 0.01-5.0%, and the sulfur content is 0-6.0%.

4. A method for preparing the modified porous amorphous carbon negative electrode material according to any one of claims 1 to 3, wherein the method include: The carbon-rich precursor is crushed to obtain carbon powder particles, and the carbon powder particles are mixed with a modifier containing at least F element for doping and modification to obtain doped carbon; The doped carbon is subjected to chemical etching to form pores to obtain porous core carbon; The core carbon is compositely coated and carbonized with amorphous carbon and conductive carbon to form a "core-shell" structure, thereby obtaining the modified porous amorphous carbon negative electrode material.

5. The preparation method according to claim 4, It is characterized in that The median particle size of the carbon powder particles is 1.5-30 μm, preferably 5-15 μm; The method for doping and modifying the carbon powder particles by mixing and reacting with a modifier containing at least the element F comprises: heating the mixture of the carbon powder particles and the modifier to react, thereby obtaining the doped carbon; if the modifier is in a gas phase, then the mixture is introduced in the form of gas; if the modifier is in a liquid phase or a solid phase, then the mixture is first mixed evenly with the carbon powder particles and then put into a reaction device for heating; preferably, the modifier further contains at least one of the elements S and N; The modifier is fluorine gas, and can also selectively react with at least one modifier selected from sulfur dioxide, sulfur trioxide, ammonia, urea, melamine, oxygen, and hydrogen peroxide; the concentration of the fluorine gas is 5-90%, preferably 10-30%; the concentration of the sulfur dioxide is 5-90%, preferably 10-50%; the concentration of the sulfur trioxide is 5-90%, preferably 10-40%; the concentration of the oxygen is 20-90%, preferably 30-50%; The doped carbon has a fluorine content of 0.01-8%, an oxygen content of 2-20%, a nitrogen content of 0-7%, and a sulfur content of 0-8%; The reaction temperature of the doping modification is 100-500°C; The reaction time of the doping modification is 1-6h; The doping modification is carried out in a reactor with stirring; The stirring rate of the stirring is 5-100 r / min, preferably 30-50 r / min.

6. The preparation method according to claim 4, It is characterized in that The chemical etching method includes gas phase etching activation and / or metal compound etching activation; The median particle size of the core carbon is 1.5-30 μm, preferably 3-15 μm; The pore size of the core carbon micropores is 0.2-2 nm, preferably 0.5-1.5 nm; The pore size of the core carbon is 2-40 nm, preferably 5-20 nm; The pore size of the macropores of the core carbon is 50-150 nm, preferably 50-100 nm; The total pore volume of the core carbon is 0.05-2.0 cm 3 / g; The specific surface area of ​​the core carbon is 1.5-50m 2 / g, preferably 5-25m 2 / g; The gas phase etching activation method comprises: heating the doped carbon in a carbon dioxide and / or water vapor atmosphere to react, thereby obtaining the core carbon; The concentration of the carbon dioxide is 1-100%, preferably 5-50%, and the balance gas is any one of nitrogen, helium, neon, argon or xenon, or a combination of at least two thereof; The water vapor introduction rate is 0.1-300 g / min, preferably 1-50 g / min; The reaction temperature of the gas phase etching activation is 400-1200°C; The reaction time of the gas phase etching activation is 0.5-6h; The gas phase etching activation is carried out in a reactor with stirring or rotation; The stirring or rotating speed is 5-100 r / min, preferably 10-50 r / min. The method for etching and activating the metal compound comprises: mixing the doped carbon and at least one selected from sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, calcium carbonate, zinc carbonate, sodium bicarbonate, potassium bicarbonate, calcium bicarbonate, iron carbonate, zinc chloride, zinc oxide, zinc acetate, sodium acetate, potassium acetate or calcium acetate, heating the mixture for reaction, and then washing with acid, washing with water and drying the mixture to obtain the core carbon; The mass ratio of the metal compound to the doped carbon is 0.02-1:1, preferably 0.05-0.5:1; The method for etching and activating the metal compound is stirring and mixing; The reaction temperature of the metal compound etching activation is 500-1400°C; The reaction time of the metal compound etching activation is 1-6h; The pickling is to mix the product obtained after the reaction with an acid in a mass ratio of 1:0.3-50, preferably 1:1-20; The pickling is carried out by using one or a combination of at least two of hydrochloric acid, nitric acid and hydrofluoric acid; The concentration of the acid is 0.5-5 mol / L; The water washing is repeated several times until the pH value of the filtrate reaches 6-7; The drying method is heating drying or supercritical drying; The ash content of the core carbon is less than 5%.

7. The preparation method according to claim 4, It is characterized in that The composite coating method in step (3) includes vapor deposition coating and / or liquid phase coating; The vapor deposition coating method comprises: subjecting the core carbon to a high-temperature carbon deposition reaction under a carbon source gas to generate an amorphous carbon coating layer on the surface of the material, and then uniformly mixing the obtained product with a conductive carbon slurry under high-speed stirring, and sintering the product through high-temperature carbonization; The carbon source is one or a combination of at least two of saturated hydrocarbons, aromatic hydrocarbons, alkenes, alkynes, alcohols, aldehydes, carboxylic acids and esters containing 1 to 8 carbon atoms, more preferably one or a combination of at least two of methane, ethane, propane, butane, ethylene, propylene, butene, acetylene, methanol, ethanol, cyclohexane, cyclopentane, toluene, xylene and aniline; The reaction temperature of the carbon deposition reaction is 700-1300°C; The carbon source introduction rate is 0.2-80 g / min, preferably 1-30 g / min; The deposition reaction is carried out in a reaction device with stirring or rotation; The liquid phase coating method comprises: uniformly mixing the core carbon with the liquid phase coating agent and the conductive carbon slurry under high-speed stirring, and then carbonizing and sintering at high temperature; The liquid coating agent is selected from one or a combination of at least two of liquid asphalt, aromatic tar, monosaccharide solution, polysaccharide solution, citric acid solution, phenolic resin solution, epoxy resin solution, polyacrylonitrile solution and polyvinyl pyrrolidone solution; the mass fraction of the solute in the solution is 5-90%, preferably 10-50%; The mass ratio of the core carbon, the amorphous carbon in the shell and the conductive carbon is 100:0.1-5:0.01-1, preferably 100:0.5-3:0.02-0.5; The conductive carbon precursor is conductive carbon slurry; The conductive carbon slurry comprises 0.01-10% conductive carbon, 0.03-3% dispersing aid and 87-99.96% solvent; The conductive carbon is one or a combination of at least two of single-walled carbon nanotubes, multi-walled carbon nanotubes, nanocarbon fibers, graphene and carbon black; The length of the carbon nanotube is 3-50 μm, preferably 5-20 μm; the diameter of the nano carbon fiber is 0.6-100 nm, and the length is 5-50 μm; the number of graphene layers is 1-50, preferably 3-10; The dispersing aid is selected from polycarboxylates, polycarboxylates, polyethylene glycols, polyfluoroolefins, polysilanes, polyacrylic acids, and silane coupling agents, and is more preferably one or a combination of at least two of carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinylidene fluoride, ethylene glycol, ethylenediaminetetraacetic acid, sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, polyethylene glycol, polysorbate-20, polysorbate-80, and polyethylene oxide-polypropylene oxide-polyethylene oxide copolymer; The solvent is selected from alcohols, ketones, esters, aromatic hydrocarbons, alicyclic hydrocarbons or water, and is more preferably one or a combination of at least two of water, ethanol, N-methylpyrrolidone, toluene and washing oil; The preparation method of the conductive carbon slurry is to add conductive carbon and a dispersing aid into a solvent and stir the mixture to obtain the conductive carbon slurry.

8. The preparation method according to claim 4, It is characterized in that The carbonization is carried out under an inert atmosphere; the inert atmosphere includes any one of a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere or a xenon atmosphere, or a combination of at least two thereof; The carbonization temperature is 800-1500°C and the time is 0.5-6h; The carbonization further comprises: cooling to 20-50° C. after sintering.

9. The preparation method according to claim 4, It is characterized in that The method for preparing the carbon powder particles comprises: crushing a carbon-rich precursor, or crushing it after low-temperature pretreatment under a suitable atmosphere to obtain the carbon powder particles; The carbon-rich precursor includes any one of coke, coal, asphalt, resin or biomass, or a combination of at least two thereof; The coke comprises any one of coal coke, petroleum coke, pitch coke, mesocarbon microbeads or charcoal, or a combination of at least two thereof; the volatile content of the coke is 0.01-15%, preferably 3-10%; The coal includes any one of anthracite, bituminous coal, sub-bituminous coal or lignite or a combination of at least two thereof; the volatile content of the coal is 0.1-50%, preferably 10-40%; the ash content of the coal is 0.001-10%, preferably 0.001-5%; The asphalt includes any one of coal tar asphalt, petroleum asphalt or shale asphalt, or a combination of at least two of them; the softening point of the asphalt is 20-350° C., preferably 150-280° C.; The resin includes any one of phenolic resin, epoxy resin, phenolic epoxy resin, furfural resin, petroleum resin, coumarone resin or polyimide resin, or a combination of at least two thereof; The appropriate atmosphere includes any one of nitrogen atmosphere, air atmosphere, oxygen atmosphere, helium atmosphere, neon atmosphere, argon atmosphere or xenon atmosphere, or a combination of at least two thereof; The biomass comprises any one or a combination of at least two of lignin, microcrystalline cellulose, starch, fruit shell, apricot shell, peach shell, coconut shell, peanut shell, rice husk, cotton husk, sawdust, bamboo fiber or straw; The temperature of the low temperature pretreatment is 200-700°C; The heating rate of the low temperature pretreatment is 0.5-20°C / min; The time of the low temperature pretreatment is 1-8h.

10. Use of the modified porous amorphous carbon negative electrode material according to claim 1 or the modified porous amorphous carbon negative electrode material prepared by the preparation method according to claim 4, It is characterized in that The modified porous amorphous carbon negative electrode material is used in lithium ion batteries, sodium ion batteries, potassium ion batteries or supercapacitors.

Citation Information

Cited By

  • Starch-based hard carbon material, preparation thereof and application of starch-based hard carbon material in sodium-ion battery

    CN119750545A

  • Silicon-carbon negative electrode material and preparation method thereof, negative electrode plate and secondary battery

    CN119864392A

  • Solid waste graphite-based base charged adsorbent and preparation method and application thereof in air carbon capture

    CN119909651A

  • Preparation method of modified coal pitch and preparation method of carbon material

    CN121379188A

  • Carbon material, preparation method therefor, use thereof, and sodium ion battery

    WO2026184217A1