Bi5O7I / Ti3C2 heterojunction catalyst and preparation method and application thereof
By preparing a Bi5O7I/Ti3C2 heterojunction catalyst and utilizing the Schottky heterojunction to suppress electron backflow, the problem of high photogenerated carrier recombination rate in antibiotic degradation by photocatalysis technology was solved, achieving efficient and stable photocatalytic degradation effect.
Patent Information
- Application Number
- CN202410841492.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing photocatalytic technologies suffer from problems such as high recombination rate of photogenerated carriers, poor light absorption performance, low photon utilization, and insufficient reaction driving force when degrading antibiotic pollutants, which limit their application in the field of pollutant removal.
A Bi5O7I/Ti3C2 heterojunction catalyst was prepared by loading Bi5O7I onto the surface of Ti3C2 through electrostatic adsorption to form a Schottky heterojunction. The zeta potential difference between Ti3C2 and Bi5O7I was utilized to suppress electron backflow and promote the separation and migration of photogenerated carriers.
It improves photocatalytic activity, significantly enhances the degradation efficiency of antibiotics under visible light, has high catalyst stability, a simple synthesis process, is safe and free of secondary pollution, and has broad application prospects.
Smart Images

Figure CN118847173B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wastewater treatment technology, specifically relating to a Bi5O7I / Ti3C2 heterojunction catalyst, its preparation method, and its application. Background Technology
[0002] Antibiotics, as an important class of antibacterial drugs, are widely used in medicine, animal husbandry, and other fields. While the use of antibiotics has brought immeasurable economic benefits, it has also caused serious environmental and ecological health problems. In recent years, due to the abuse and misuse of antibiotics, most antibiotics that are not metabolized by organisms are directly excreted in the form of parent compounds. Excessive levels of antibiotics have been repeatedly detected in surface water, groundwater, sewage treatment plants, and soil worldwide. Furthermore, antibiotics are not easily degraded by microorganisms or natural light, and conventional wastewater treatment systems cannot completely remove them, easily accumulating in water bodies and soil, inducing antibiotic resistance genes, and causing serious harm to ecological security and human health. In past research, many methods have been used to remove antibiotic pollutants, including filtration, adsorption, advanced oxidation, biodegradation, and photocatalytic degradation. Among these methods, photocatalytic degradation can be considered an effective and environmentally friendly approach.
[0003] However, photocatalysis technology suffers from drawbacks such as high recombination rate of photogenerated carriers, poor light absorption performance, low photon utilization, and insufficient reaction driving force, which greatly limits its application in pollutant removal. To improve the photocatalytic activity of catalysts and enhance the application of photocatalysis technology in the environmental field, researchers have proposed various modification methods, such as elemental doping, defect engineering, morphology control, and heterojunction construction. Among these, heterojunction construction is a simple and efficient method. The energy barrier of Schottky heterojunctions effectively inhibits the backflow of photogenerated electrons to the catalyst, enabling efficient unidirectional transfer of photogenerated carriers through the interface, thereby suppressing the recombination efficiency of photogenerated carriers. Using Schottky heterojunction catalysts to remove antibiotic pollution from water bodies offers advantages such as being green, efficient, and safe. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a Schottky heterojunction catalyst with high catalytic efficiency, high stability, and environmental friendliness, a simple method for preparing the catalyst, and its application in degrading organic pollutants in water.
[0005] A Bi5O7I / Ti3C2 heterojunction catalyst is provided, wherein Bi5O7I is loaded onto the Ti3C2 surface with a zeta potential opposite to that of Bi5O7I via electrostatic adsorption; the catalyst has a Schottky heterojunction that suppresses electron backflow; and the catalyst is a nanosheet.
[0006] Furthermore, the mass ratio of Ti3C2 to Bi5O7I is 0.1~2%.
[0007] A method for preparing the above-mentioned Bi5O7I / Ti3C2 heterojunction catalyst includes the following steps:
[0008] a) Dissolve bismuth nitrate in a 0.1-0.5 M dilute nitric acid solution to obtain solution A; uniformly disperse potassium iodide and hexadecyltrimethylammonium bromide in water to obtain solution B;
[0009] b. Slowly add solution A to solution B, adjust the pH of the mixed solution to alkaline and maintain it at 100-150 °C for 10-24 h; separate and collect the precipitate, wash it with ethanol and water until neutral, and dry it to obtain Bi5O7I precursor; calcine the dried Bi5O7I precursor at 450-500 °C for 2-4 h to obtain Bi5O7I;
[0010] c. Disperse Bi5O7I and Ti3C2 in water to obtain Bi5O7I dispersion and Ti3C2 dispersion respectively; add Ti3C2 dispersion dropwise to Bi5O7I dispersion, stir at room temperature for 8-12 h, separate and collect the precipitate and dry it to obtain Bi5O7I / Ti3C2 heterojunction catalyst.
[0011] Furthermore, the concentration of bismuth nitrate in solution A in step a is 0.25~1.8 mmol / mL; the concentration of potassium iodide in solution B in step a is 0.025~0.1 mmol / mL.
[0012] Furthermore, in step a, the mass ratio of potassium iodide to hexadecyltrimethylammonium bromide is 1:(1~1.2); and the molar ratio of potassium iodide to bismuth nitrate is 1:1.
[0013] The preparation method of the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 3 is characterized in that the alkaline pH in step b is 9~11; and the calcination heating rate is 2~5 ℃ / min.
[0014] Furthermore, step c, which involves collecting the precipitate by centrifugation and then drying it at 60℃~80℃ for 12~24h, is a further step.
[0015] Furthermore, the preparation of the Ti3C2 includes the following steps:
[0016] Ti3AlC2 was dispersed in hydrofluoric acid solution and stirred continuously; the solid was collected, washed with water until neutral, and dried thoroughly; the dried solid was placed in dimethyl sulfoxide solution and stirred continuously for 48-72 h; then placed in water and sonicated continuously under N2 atmosphere for 5-10 h, and centrifuged to obtain Ti3C2.
[0017] Furthermore, the concentration of the hydrofluoric acid solution is 20-40%, and it is continuously stirred for 5-7 days.
[0018] The above-mentioned Bi5O7I / Ti3C2 heterojunction catalyst is applied in water pollution control, degrading organic pollutants under light irradiation.
[0019] By adopting the above scheme, the method of the present invention has the following advantages:
[0020] 1. The Bi5O7I of this invention has an opposite zeta potential to Ti3C2, and it can form a heterojunction catalyst through electrostatic attraction. Compared with traditional deposition methods, the heterojunction formed by electrostatic attraction in this invention has better stability, and the 2D structure of the material results in higher interfacial bonding.
[0021] 2. The heterojunction catalyst of the present invention has excellent photocatalytic activity and can effectively degrade antibiotics in water under visible light irradiation.
[0022] 3. The energy barrier in the Schottky heterojunction of the present invention makes it difficult for e‾ on the Ti3C2 surface to flow back to Bi5O7I, which can effectively hinder the backflow of photogenerated electrons, promote the separation of photogenerated charge carriers, suppress the photocorrosion of the catalyst, and improve the photocatalytic activity.
[0023] 4. The 2D / 2D contact mode between Bi5O7I and Ti3C2 in the catalyst of the present invention can shorten the migration distance and migration time of photogenerated carriers, promote the migration of photogenerated carriers to the catalyst surface, and result in higher photocatalytic activity.
[0024] 5. The synthesis process of this invention is simple and easy to operate, the reaction conditions are easy to achieve, the safety is high, there is no excessive addition of non-product elements, the product has high purity and few impurities, there is no secondary pollution, and the application prospects are broad. Attached Figure Description
[0025] Figure 1 These are the X-ray diffraction (XRD) patterns of Examples 1-5.
[0026] Figure 2 This is a transmission electron microscope (TEM) image of Comparative Example 1.
[0027] Figure 3 This is a transmission electron microscope (TEM) image of Comparative Example 2.
[0028] Figure 4 This is a transmission electron microscope (TEM) image of Example 1.
[0029] Figure 5 This is a comparison diagram of the UV-Vis diffuse reflectance spectra of Example 1 and Comparative Examples 1 and 2.
[0030] Figure 6 These are comparison diagrams showing the visible light catalytic degradation effect of CIP in water in Examples 1-3 and Comparative Examples 1 and 2.
[0031] Figure 7 This is Example 1, showing the degradation of CIP in water after adding a free radical scavenger during the visible light catalytic degradation process.
[0032] Figure 8 This is a control diagram of the visible light photocatalytic degradation of CIP cycle in water in Example 1.
[0033] Figure 9 This is a schematic diagram of the mechanism of visible light catalytic degradation of antibiotics in water using Example 1. Detailed Implementation
[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0035] Example 1:
[0036] (1) 2D Bi5O7I was prepared by hydrothermal assisted calcination; 3 mmol of bismuth nitrate pentahydrate was ultrasonically dissolved in 5 mL of dilute nitric acid solution (0.3 M), and the solution was named solution A; 3 mmol of potassium iodide and 0.5 g of hexadecyltrimethylammonium bromide were uniformly dispersed in 60 mL of deionized water, and the solution was named solution B.
[0037] (2) Solution A was slowly added dropwise to solution B, the pH of the mixed solution was adjusted to 9 and kept at 120 °C for 12 h; the BiOI precursor was collected by filtration, washed with anhydrous ethanol and ultrapure water until neutral, and dried at 60 °C for 24 h; the dried BiOI precursor was placed in a muffle furnace and calcined at 450 °C for 2 h with a heating rate of 5 °C / min to obtain Bi5O7I.
[0038] (3) Ti3C2 was prepared by hydrofluoric acid etching and ultrasonic stripping. 1 g of Ti3AlC2 was placed in 40% hydrofluoric acid solution and stirred continuously for 7 days. The solid was collected, washed with ultrapure water until neutral, and dried under vacuum at 60 °C for 24 h. The dried solid was placed in dimethyl sulfoxide solution and stirred continuously for 72 h. The solid from step 3 was placed in ultrapure water and ultrasonically treated under N2 conditions for 10 h. After centrifugation, Ti3C2 was obtained.
[0039] (4) Synthesis of heterojunction catalyst by electrostatic adsorption: 0.2 g Bi5O7I was ultrasonically dispersed in ultrapure water, and Ti3C2 solution was added dropwise to the above solution. The mixture was stirred at room temperature for 8 h, centrifuged, and dried at 60 ℃ for 12 h to obtain Bi5O7I / Ti3C2 catalyst. The mass ratio of Ti3C2 to Bi5O7I was 0.5%, and it was named BT-0.5.
[0040] Example 2:
[0041] The difference from Example 1 is that the mass ratio of Ti3C2 to Bi5O7I is 0.1%, and it is named BT-0.1.
[0042] Example 3:
[0043] The difference from Example 1 is that the mass ratio of Ti3C2 to Bi5O7I is 2%, and it is named BT-2.
[0044] Comparative Example 1:
[0045] 3 mmol of bismuth nitrate pentahydrate was ultrasonically dissolved in 5 mL of dilute nitric acid solution (0.3 M), and this solution was named solution A. Then, 3 mmol of potassium iodide and 0.5 g of hexadecyltrimethylammonium bromide were uniformly dispersed in 60 mL of deionized water, and this solution was named solution B. Solution A was then slowly added dropwise to solution B, and the pH of the mixed solution was adjusted to 9 and maintained at 120 °C for 12 h. The BiOI precursor was collected by filtration, washed with anhydrous ethanol and ultrapure water until neutral, and dried at 60 °C for 24 h. Finally, the dried BiOI precursor was placed in a muffle furnace and calcined at 450 °C for 2 h at a heating rate of 5 °C / min to obtain the Bi5O7I catalyst, named BOI.
[0046] Comparative Example 2:
[0047] 1 g of Ti3AlC2 was placed in a 40% hydrofluoric acid solution and stirred continuously for 7 days. The solid was collected, washed with ultrapure water until neutral, and dried under vacuum at 60 °C for 24 h. Subsequently, the dried solid was placed in a dimethyl sulfoxide solution and stirred continuously for 72 h. Finally, the solid from step 3 was placed in ultrapure water and subjected to continuous ultrasonic treatment under N2 conditions for 10 h. After centrifugation, the Ti3C2 catalyst was obtained.
[0048] Example Sample Testing:
[0049] Figure 1 These are the XRD patterns of the catalysts (BOI, Ti3C2, BT-0.1, BT-0.5, and BT-2) from Examples 1-3 and Comparative Examples 1 and 2, respectively. Figure 1It can be seen that BOI (i.e., Bi5O7I) has six typical crystal planes, namely (200), (312), (113), (004), (204), and (020). Ti3C2 has five typical crystal planes, namely (004), (006), (008), (010), and (110). The XRD patterns of BT-0.1, BT-0.5, and BT-2 are similar to those of BOI, and the diffraction peak intensity of the (113) crystal plane gradually increases with the increase of Ti3C2 content.
[0050] Figure 2 , Figure 3 and Figure 4 The images show TEM images of the BOI catalyst of Comparative Example 1, the Ti3C2 catalyst of Comparative Example 2, and the BT-0.5 catalyst of Example 1, respectively. The TEM images show that Bi5O7I / Ti3C2 and Ti3C2 are both nanosheet structures, and Bi5O7I / Ti3C2 is a superposition of two kinds of nanosheets.
[0051] The UV-Vis diffuse reflectance properties of Example 1 and Comparative Examples 1 and 3 were tested, and the results are as follows: Figure 5 As shown, all three materials exhibit excellent light absorption for both ultraviolet and visible light. The light absorption performance of Bi5O7I / Ti3C2 is significantly higher than that of Bi5O7I, indicating that the introduction of Ti3C2 material can effectively improve the light absorption performance and light utilization rate of Bi5O7I.
[0052] Test of visible light photocatalytic degradation of CIP in water: 50 mg of each catalyst sample from the examples and comparative examples were added to 50 mL of a 10 mg / L CIP solution. The mixtures were placed in the dark at 30°C and 500 rpm for 60 min until adsorption-desorption equilibrium was reached. Then, the mixtures were placed under a xenon lamp (λ > 420 nm) for photocatalytic reaction at 30°C for 60 min and a stirring rate of 500 rpm.
[0053] Figure 6 This is a comparison chart of the visible light photocatalytic degradation effects of various photocatalytic materials on CIP in water. Figure 6 It can be seen that, compared with Bi5O7I, the Bi5O7I / Ti3C2 photocatalytic material significantly improves the degradation effect of CIP, among which Bi5O7I / Ti3C2 has the highest photocatalytic activity, and the degradation rate of CIP can reach 96.7%.
[0054] The generation of free radicals during the degradation of CIP: 50 mg each of the Bi5O7I / Ti3C2 catalyst from Example 1 was added to three separate 50 mL CIP solutions with a concentration of 10 mg / L. Each mixture was placed in the dark at 30°C and 500 rpm for 60 min until adsorption-desorption equilibrium was reached. Then, 1 mM trihydroxyethylamine (TEA-h) was added to each solution. + ), 1 mM p-benzoquinone (BQ-·O2) − The mixture was prepared with 1 mM isopropanol (IPA-·OH) and then placed under a xenon lamp (λ > 420 nm) for photocatalytic reaction. The reaction system was heated to 30 °C, the illumination time was 60 min, and the solution stirring rate was 500 rpm.
[0055] Figure 7 These are the degradation rates of CIP in water under visible light catalytic degradation by Bi5O7I / Ti3C2 in Example 1, after the addition of a scavenging agent. Figure 7 It can be seen that compared with the absence of a free radical scavenger, the degradation rate of CIP decreased after the addition of the scavenger, indicating that the three free radicals (h) + , O2 − O2 plays an important role in the photodegradation of TCH, particularly ·OH. − It has the greatest effect on the degradation of CIP, followed by h. + Then, ·OH.
[0056] Stability test of visible light photocatalytic degradation of antibiotics in water: 50 mg of Bi5O7I / Ti3C2 from Example 1 was added to 50 mL of a 10 mg / L CIP solution. The mixture was placed in the dark at 30°C and 500 rpm for 60 min until adsorption-desorption equilibrium was reached. Then, the mixture was placed under a xenon lamp (λ > 420 nm) for photocatalytic reaction at 30°C for 60 min and a stirring rate of 500 rpm. After degradation, the mixture was centrifuged at 8000 rpm, the supernatant was removed, and 50 mL of CIP solution (10 mg / L) was added. The degradation experiment was repeated four times, and the degradation efficiency of the Bi5O7I / Ti3C2 photocatalyst for antibiotics was measured each time.
[0057] Figure 8 This is a control diagram of the Bi5O7I / Ti3C2 photocatalytic degradation of CIP cycle in water in Example 1. Figure 8It can be seen that after four cycles of the experiment, the degradation efficiency of the Bi5O7I / Ti3C2 photocatalyst for antibiotics decreased slightly, but it still showed good degradation effect, indicating that the Bi5O7I / Ti3C2 photocatalyst has good stability.
[0058] The mechanism of visible light photocatalytic degradation of antibiotics in water using the catalyst of Example 1 Figure 9 As shown, the work functions of Bi5O7I and Ti3C2 in the catalyst of this invention are 5.505 eV and 6.354 eV, respectively. The difference in work function indicates a difference in Fermi levels. When Bi5O7I comes into contact with Ti3C2, electrons can transfer from Bi5O7I to Ti3C2, resulting in an electron accumulation layer on the Ti3C2 contact surface and a consumption layer on the Bi5O7I contact surface. Simultaneously, the Fermi levels of Bi5O7I and Ti3C2 shift, i.e., the Fermi level of Bi5O7I shifts downwards and the Fermi level of Ti3C2 shifts upwards, until the Fermi levels reach equilibrium. This Fermi level migration causes the energy band of Bi5O7I to bend upwards. The potential difference at the contact surface between Bi5O7I and Ti3C2 leads to the formation of a built-in electric field, with the direction of the electric field pointing from Ti3C2 to Bi5O7I. When the catalyst is irradiated under visible light, Bi5O7I can generate photogenerated electrons (e‾) and photogenerated holes (h‾). + Driven by the built-in electric field, electrons migrate from the conduction band of Bi5O7I to the Ti3C2 surface and react with O2 to generate superoxide radicals (•O2). Due to the Schottky barrier, electrons on the Ti3C2 surface do not easily flow back to Bi5O7I, thus inhibiting the recombination of photogenerated carriers. The h-values on the valence band of Bi5O7I... + It can oxidize OH⁻ adsorbed on the catalyst surface to generate •OH⁻. •O₂⁻, h + It works in conjunction with •OH to break down organic pollutants into smaller molecules and eventually mineralize them into CO2 and H2O.
[0059] For those skilled in the art, various other corresponding changes and modifications can be made based on the technical solutions and concepts described above, and all such changes and modifications should fall within the protection scope of the claims of this invention.
Claims
1. A method for preparing a Bi5O7I / Ti3C2 heterojunction catalyst, characterized in that, Bi5O7I is loaded onto the Ti3C2 surface with a zeta potential opposite to that of Bi5O7I through electrostatic adsorption; the catalyst has a Schottky heterojunction that suppresses electron backflow. The catalyst is a nanosheet; the preparation method of the catalyst includes the following steps: a) Dissolve bismuth nitrate in a 0.1-0.5 M dilute nitric acid solution to obtain solution A; uniformly disperse potassium iodide and hexadecyltrimethylammonium bromide in water to obtain solution B; b. Slowly add solution A to solution B, adjust the pH of the mixed solution to alkaline and maintain it at 100-150 °C for 10-24 h; separate and collect the precipitate, wash it with ethanol and water until neutral, and dry it to obtain Bi5O7I precursor; calcine the dried Bi5O7I precursor at 450-500 °C for 2-4 h to obtain Bi5O7I; c. Disperse Bi5O7I and Ti3C2 in water to obtain Bi5O7I dispersion and Ti3C2 dispersion respectively; add Ti3C2 dispersion dropwise to Bi5O7I dispersion so that the mass ratio of Ti3C2 to Bi5O7I is 0.1~2%; stir at room temperature for 8~12h; separate and collect the precipitate and dry it to obtain Bi5O7I / Ti3C2 heterojunction catalyst.
2. The preparation method of the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 1, characterized in that, The concentration of bismuth nitrate in solution A in step a is 0.25~1.8 mmol / mL; the concentration of potassium iodide in solution B in step a is 0.025~0.1 mmol / mL.
3. The preparation method of the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 1, characterized in that, The mass ratio of potassium iodide to hexadecyltrimethylammonium bromide in step a is 1:(1~1.2); the molar ratio of potassium iodide to bismuth nitrate is 1:
1.
4. The preparation method of the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 1, characterized in that, The alkaline pH in step b is 9-11; the heating rate during calcination is 2-5 °C / min.
5. The method for preparing the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 1, characterized in that, Step c describes separating, collecting, and drying the precipitate by centrifuging and then drying it at 60℃~80℃ for 12~24h.
6. The method for preparing the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 1, characterized in that, The preparation of the Ti3C2 includes the following steps: Ti3AlC2 was dispersed in hydrofluoric acid solution and stirred continuously; the solid was collected, washed with water until neutral, and dried thoroughly; the dried solid was placed in dimethyl sulfoxide solution and stirred continuously for 48-72 h; then placed in water and sonicated continuously under N2 atmosphere for 5-10 h, and centrifuged to obtain Ti3C2.
7. The method for preparing the Bi5O7I / Ti3C2 heterojunction catalyst according to claim 6, characterized in that, The concentration of the hydrofluoric acid solution is 20-40%, and it is stirred continuously for 5-7 days.
8. The application of the Bi5O7I / Ti3C2 heterojunction catalyst prepared by the method of claim 1 in water pollution treatment, characterized in that, Organic pollutants decompose under sunlight.
Citation Information
Patent Citations
2D / 2DBiOI / Ti3C2 composite photocatalyst as well as preparation method and application thereof
CN111632615A
Two-dimensional porous Bi5O7I nanosheet photocatalyst and preparation method thereof
CN113952967A