Nanometer silicon, preparation method and application thereof and lithium ion battery

Nano-silicon is prepared by reducing sodium silicon-selenide compounds with metallic sodium, which solves the problems of poor reaction controllability and difficult removal of impurities in the magnesia-thermal reduction method. It achieves mild preparation and high performance of nano-silicon, and has high performance when used in lithium-ion battery negative electrodes. specific capacity and long cycle life.

CN118851179APending Publication Date: 2024-10-29无锡锂凰科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410854669.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the process of preparing silicon by magnesium thermal reduction method in the prior art, the reaction controllability is poor, the silicon structure is easily destroyed, and the generated impurities are difficult to remove, which limits the preparation of nano-silicon materials and the performance of lithium-ion batteries.

Method used

Nano-silicon materials are prepared by reducing sodium silicon-selenide compounds with metallic sodium. By heating the mixture of Na and Na2SiSe3 at 80°C to 300°C, the strong reducing properties of metallic sodium are used to achieve mild and controllable preparation of nano-silicon, and the by-products are processed through dissolution and distillation. The product sodium selenide avoids the problem of difficult separation of impurities.

Benefits of technology

It achieves high specific capacity and cycle stability of nano-silicon materials, overcomes the problems of difficult-to-control product morphology and reaction rate caused by violent reactions and high exothermic characteristics in traditional methods, and prepares small-sized nano-silicon particles for Lithium-ion batteries have high specific capacity and long cycle life when used as the negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851179A_ABST
    Figure CN118851179A_ABST
Patent Text Reader

Abstract

The invention discloses nano silicon, a preparation method and application thereof and a lithium ion battery. The method comprises the following steps: heating a mixture of metal Na and Na2SiSe3 for 1-18 hours at the temperature of 80-300 DEG C under the protection of inert gas, cooling, washing and drying to obtain the nano silicon, the molar ratio of the metal Na to the Na2SiSe3 is (4 to 5): 1. According to the preparation method provided by the invention, the problem that the product morphology and the reaction rate are difficult to control due to violent traditional magnesiothermic reduction reaction and high exothermic characteristic is solved, and mild and controllable preparation of the nano silicon material can be realized. The prepared nano silicon particles are small in size, and have the characteristics of high specific capacity, high cycle and the like when being used for the negative electrode of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to nano silicon and a preparation method, application and lithium ion battery thereof. Background Art

[0002] The main function of the negative electrode material of lithium-ion batteries is to store and release lithium ions while maintaining the stability of the electrode structure. During the battery charging and discharging process, lithium ions move back and forth between the positive and negative electrodes, and the negative electrode material plays a key role in this process. Therefore, the research on negative electrode materials is of great significance to improving the performance and safety of lithium-ion batteries. At present, commercial lithium-ion batteries mainly use carbon-based negative electrode materials, such as graphite. Graphite negative electrode has the advantages of good electrochemical properties, cycle stability and low cost, but its energy density and power density are relatively low, which limits its application in high energy density batteries and fast charging and discharging scenarios.

[0003] In order to further improve the performance of lithium-ion batteries, silicon-based materials, tin-based materials, nitrides, phosphates, etc. are gradually applied to negative electrode materials. Among them, silicon, as a new type of negative electrode material, has a high theoretical specific capacity of about 4200mAh / g, which is much higher than the 372mAh / g of traditional graphite negative electrode; at the same time, it has good cycle stability, low discharge potential, and rich content, which is conducive to large-scale production and cost reduction. Therefore, it is considered to be a negative electrode material with great application potential. However, silicon negative electrode materials have serious volume expansion during the charging and discharging process (up to more than 300%), which leads to electrode structure destruction, conductive network failure and decreased cycle stability. In addition, the intrinsic conductivity of silicon negative electrode materials is poor, resulting in limited power density and charge and discharge rate of the electrode. Due to problems such as volume expansion and poor conductivity, the cycle stability of silicon negative electrode materials is poor, which limits their life in practical applications.

[0004] At present, commercial nano silicon negative electrode materials are produced by reducing the size of silicon particles to nanometer scale, increasing the specific surface area, which is beneficial to lithium storage, increasing the specific capacity and alleviating the volume expansion problem of silicon during the charge and discharge process, thereby improving the cycle stability of the battery. However, the current industrial preparation methods of nano silicon such as sand grinding, vapor deposition, and evaporation have extremely high requirements for equipment, and have problems such as low production efficiency, difficult equipment maintenance, and limited output. Therefore, it is very important to develop a low-cost controllable solid-phase synthesis method to prepare nano silicon.

[0005] Metal reduction can be used to synthesize silicon. For example, crude silicon is often reduced to silicon dioxide with magnesium at high temperature to generate silicon dioxide, which has the advantages of low cost, fast reaction, and high yield. However, the reaction of magnesium and other metals to reduce silicon dioxide has poor controllability, is prone to large amounts of heat release, and destroys the silicon micro-nano structure. In addition, impurities such as magnesium oxide are generated, which are difficult to remove. Summary of the invention

[0006] The technical problem solved by the present invention is to overcome the defects of poor reaction controllability, easy destruction of silicon structure and difficulty in removing generated impurities in the conventional magnesium thermal reduction method in the prior art, and provide nano silicon and its preparation method, application and lithium ion battery. The preparation method of the present invention can realize mild and controllable preparation of nano silicon materials, easy removal of impurities, and the prepared nano silicon material is small in size and has high specific capacity, high cycle and other characteristics when used for the negative electrode of lithium ion batteries.

[0007] The present invention prepares nano silicon material by reducing sodium silicon selenide compounds with metallic sodium. This method utilizes the stronger reducing property of metallic sodium, overcomes the problem that the product morphology and reaction rate are difficult to control due to the violent and highly exothermic characteristics of the traditional magnesium thermal reduction reaction, and can realize the gentle and controllable preparation of nano silicon material. In addition, the reaction byproduct sodium selenide can be dissolved and recycled after distillation, effectively avoiding the process difficulty that the traditional oxide byproduct is difficult to separate and must be removed by acid washing and other methods. This method can prepare nano silicon particles with smaller size, which have the characteristics of high specific capacity and high cycle when used for the negative electrode of lithium ion batteries.

[0008] The present invention solves the above technical problems through the following technical solutions:

[0009] The present invention provides a method for preparing nano-silicon, which comprises the following steps:

[0010] The metal Na and Na 2 SiSe 3 The mixture is heated at 80°C to 300°C for 1-18h under the protection of an inert gas, and then washed and dried after cooling to obtain the nano-silicon; the metal Na and the Na 2 SiSe 3 The molar ratio is (4-5):1.

[0011] In the present invention, the Na 2 SiSe 3 It can be obtained from conventional commercial sources or prepared by itself. 2 SiSe 3 The preparation method preferably comprises the following steps:

[0012] The mixture of sodium selenide, silicon powder and selenium powder is kept at 700-1000° C. for 1-6 hours by high-temperature solid phase reaction method under the protection of inert gas, and then cooled.

[0013] According to the conventional art, the main component of the silicon powder is silicon dioxide, the mesh size of the silicon powder can be 40-200 meshes, and the mesh size of the selenium powder can be 200-500 meshes, for example, 350 meshes.

[0014] Wherein, the molar ratio of the sodium selenide, the silicon powder and the selenium powder is generally 1:1:2.

[0015] The insulation temperature is preferably 800-900° C., such as 850° C. The insulation time is preferably 2-4 hours, such as 3 hours.

[0016] In the present invention, the inert gas may be a conventional industrial inert gas, such as nitrogen or argon.

[0017] In the present invention, according to the convention in the art, the heating and the high-temperature solid-phase reaction are generally performed in a tube furnace.

[0018] In the present invention, the rate of heating to the heating temperature may be 2-5°C / min, for example 3°C / min.

[0019] In the present invention, the heating temperature may be, for example, 85°C, 120°C, 130°C, 140°C, 200°C or 280°C, preferably 80-100°C.

[0020] In the present invention, the heating time may be, for example, 1.5 h, 3 h, 4 h, 6 h or 10 h, preferably 2-6 h.

[0021] In the present invention, the metal Na and the Na 2 SiSe 3 The molar ratio is preferably (4-4.5):1, such as 4:1, 4.2:1 or 4.5:1, more preferably (4.3-4.5):1.

[0022] In the present invention, the solvent used for washing can be one or more of DMF, NMP and DMSO, preferably DMF. The solution separated after washing can be recovered by distillation to obtain high-purity Na 2 Se, can be used for Na 2 SiSe 3 Circular preparation or sale.

[0023] In the present invention, the drying operation and conditions may be conventional in the art, such as drying.

[0024] The present invention also provides nano silicon prepared by the method as described above.

[0025] In the present invention, the nano-silicon may be in the form of particles. The particle size D of the nano-silicon is 50 It can be 10-300nm, preferably 100-300nm.

[0026] In the present invention, the specific capacity of the negative electrode of the nano-silicon used in lithium-ion batteries is preferably greater than 1500 mAh / g.

[0027] The present invention also provides an application of the nano silicon as described above in a lithium ion battery.

[0028] The present invention also provides a lithium ion battery, which comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the negative electrode comprises the nano-silicon as described above.

[0029] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0030] The reagents and raw materials used in the present invention are commercially available.

[0031] The positive and progressive effects of the present invention are:

[0032] The present invention overcomes the problem that the product morphology and reaction rate are difficult to control due to the violent and highly exothermic characteristics of the traditional magnesium thermal reduction reaction. The highly reducing metal sodium can be used to achieve the controllable preparation of nano-silicon materials at a lower temperature; and in addition, the reaction by-product sodium selenide can be dissolved and separated from the nano-silicon, and recycled after distillation. Through this low-temperature reduction method, smaller nano-silicon particles can be prepared, which have the characteristics of high specific capacity and high cycle when used for the negative electrode of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the SEM image of nano-silicon prepared in Example 1;

[0034] Figure 2 This is the SEM image of the silicon material prepared in Comparative Example 1;

[0035] Figure 3 This is the XRD pattern of nano-silicon prepared in Example 1. DETAILED DESCRIPTION

[0036] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0037] Example 1

[0038] (1) Sodium selenide powder (Sigma-Aldrich, purity > 95%), high purity silicon powder (purity > 99%, Aladdin, 40-200 mesh) and selenium powder (Adamas, purity 99.5%, 350 mesh) were mixed in a molar ratio of 1:1:2 and heated to 850°C in an argon-protected tube furnace for 3 hours and then naturally cooled to room temperature to obtain amorphous Na 2 SiSe 3 ;

[0039] (2) Metal Na powder (purity 99.5%, Tongguang Fine Chemical Co., Ltd.) and Na 2 SiSe3 The mixture was mixed in a crucible at a molar ratio of 4.2:1, and heated to 120°C at 3°C / min in a tube furnace protected by high-purity argon. After being kept warm for 4 hours, the mixture was naturally cooled to room temperature. The reaction product was washed with DMF solvent, filtered and dried to obtain nano-silicon material. The solvent after washing and filtration was distilled to obtain high-purity Na 2 Se.

[0040] Example 2

[0041] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The molar ratio was changed to 4:1, and the other parameters and conditions were the same as those in Example 1.

[0042] Example 3

[0043] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The molar ratio was changed to 4.5:1, and the other parameters and conditions were the same as those in Example 1.

[0044] Example 4

[0045] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The heating reaction temperature was changed to 85°C, and the other parameters and conditions were the same as those in Example 1.

[0046] Example 5

[0047] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The heating reaction temperature was changed to 200° C., and the other parameters and conditions were the same as those in Example 1.

[0048] Example 6

[0049] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The heating reaction temperature was changed to 280°C, and the other parameters and conditions were the same as those in Example 1.

[0050] Example 7

[0051] Compared with Example 1, in addition to adding metallic sodium powder and Na 2 SiSe 3 The heating reaction time was changed to 10 h, and the other parameters and conditions were the same as those in Example 1.

[0052] Example 8

[0053] Compared with Example 1, in addition to adding metallic sodium powder and Na2 SiSe 3 The heating reaction time was changed to 1.5 h, and the other parameters and conditions were the same as those in Example 1.

[0054] Example 9

[0055] (1) Sodium selenide powder (Sigma-Aldrich, purity > 95%), high purity silicon powder (purity > 99%, Aladdin, 40-200 mesh) and selenium powder (Adamas, purity 99.5%, 350 mesh) were mixed in a molar ratio of 1:1:2 and heated to 850°C in an argon-protected tube furnace for 3 hours and then naturally cooled to room temperature to obtain amorphous Na 2 SiSe 3 ;

[0056] (2) Metal Na powder (purity 99.5%, Tongguang Fine Chemical Co., Ltd.) and Na 2 SiSe 3 The mixture was mixed in a crucible at a molar ratio of 4.5:1, and heated to 85°C at 3°C / min in a tube furnace protected by high-purity argon. After being kept warm for 4 hours, the mixture was naturally cooled to room temperature. The reaction product was washed with DMF solvent, filtered and dried to obtain nano-silicon material. The solvent after washing and filtration was distilled to obtain high-purity Na 2 Se.

[0057] Comparative Example 1

[0058] Magnesium powder and silicon dioxide powder (3AChem, size 1-3μm, purity 99.9%) were placed in a crucible at a molar ratio of 1:0.48, and then heated to 500°C at 5°C / min in a high-purity argon atmosphere in a tube furnace, kept warm for 4 hours, and then cooled to room temperature. The product was washed with 0.5M dilute hydrochloric acid, 1%wt hydrofluoric acid, and a mixed solution of water and ethanol in a volume ratio of 1:1, respectively, and dried to obtain silicon material.

[0059] Effect Example

[0060] (1) Morphology characterization and XRD testing

[0061] Figure 1 This is a SEM image of the nano-silicon prepared in Example 1; Figure 2 This is a SEM image of the silicon prepared in Comparative Example 1. It can be seen that the size of the nano-silicon in Example 1 is significantly smaller than that in Comparative Example 1. Figure 3 This is the XRD pattern of the nano-silicon prepared in Example 1, and its composition is Si.

[0062] The particle sizes of the nano-silicon prepared in Examples 1-9 and Comparative Example 1 were statistically analyzed using a laser particle size distribution analyzer MS3000, as shown in Table 1:

[0063] Table 1

[0064]

[0065]

[0066] (2) EDS: The prepared amorphous Na 2 SiSe 3 EDS characterization was performed, and the element composition tested by EDS was consistent with the element feed ratio, thus confirming that the amorphous Na 2 SiSe 3 specific molecular composition.

[0067] (3) Electrochemical performance test

[0068] The nano-silicon materials prepared in Examples 1 to 9 and Comparative Example 1 were subjected to half-cell tests. The test method is: the nano-silicon materials were uniformly mixed with a binder, CMC (sodium carboxymethyl cellulose), and conductive carbon black in a mass ratio of 80:10:10, and the slurry was coated on a copper foil with a coating thickness of 100 microns, and then dried at 80°C in vacuum for 12 hours to prepare a negative electrode sheet for a lithium battery. The simulated battery assembly was carried out in an argon-filled glove box, using 1 mol / L LiPF 6 The electrolyte (solvents are EC, DMC and FEC, EC:DMC=1:1 (volume ratio), FEC accounts for 5% of the total volume of the solvent), polypropylene microporous membrane as the separator, metal lithium sheet as the counter electrode, and the electrochemical performance test is carried out on a Land CT2001A battery tester at 20 °C. The charge and discharge voltage range is 0.01 to 1.5 V (1C=250 mAh g -1 ). The test results are shown in Table 2.

[0069] Table 2

[0070]

[0071]

[0072] According to the above experimental results, it can be seen that the nano-silicon material prepared by the present invention has excellent electrochemical properties, especially specific capacity and cycle life.

[0073] In Comparative Example 1, during the preparation process, direct reduction of silicon dioxide by metallic magnesium will release high heat in a short time to destroy the silicon micro-nano structure, resulting in larger product particles, increased specific surface area, and reduced specific capacity. Compared with nano-silicon, the silicon expansion and differentiation problem is more serious, so the electrochemical performance is poor, and the first charge capacity and cycle performance are far worse than those in the embodiment.

[0074] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.

Claims

1. A method for preparing nano-silicon, characterized in that: It includes the following steps: The mixture of metal Na and Na2SiSe3 is heated at 80°C to 300°C for 1-18h under the protection of inert gas, and then washed and dried after cooling to obtain the nano-silicon; the molar ratio of the metal Na to the Na2SiSe3 is (4-5):

1.

2. The method for preparing nano-silicon according to claim 1, characterized in that: The heating temperature is 85°C, 120°C, 130°C, 140°C, 200°C or 280°C, preferably 80-100°C.

3. The method for preparing nano-silicon according to claim 1, characterized in that: The heating time is 1.5 h, 3 h, 4 h, 6 h or 10 h, preferably 2-6 h.

4. The method for preparing nano-silicon according to claim 1, characterized in that: The molar ratio of the metal Na to the Na2SiSe3 is (4-4.5):1, such as 4:1, 4.2:1 or 4.5:1, preferably (4.3-4.5):

1.

5. The method for preparing nano-silicon according to claim 1, characterized in that: The solvent used for the washing is one or more of DMF, NMP and DMSO, preferably DMF.

6. The method for preparing nano-silicon according to claim 1, characterized in that: The preparation method of Na2SiSe3 comprises the following steps: The mixture of sodium selenide, silicon powder and selenium powder is kept at 700-1000° C. for 1-6 hours by high-temperature solid phase reaction method under the protection of inert gas, and then cooled.

7. The method for preparing nano-silicon according to claim 6, characterized in that: The mesh number of the silicon powder is 40-200 mesh; And / or, the mesh size of the selenium powder is 200-500 mesh; And / or, the insulation temperature is 800-900°C; And / or, the insulation time is 2-4h.

8. A nano-silicon, characterized in that: It is prepared according to the method for preparing nano silicon according to any one of claims 1 to 7; Wherein, the particle size D of the nano silicon 50 Preferably it is 10-300nm.

9. Use of the nano-silicon as claimed in claim 8 in lithium-ion batteries.

10. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the negative electrode comprises the nano-silicon as claimed in claim 8.