CT (Computed Tomography) developable paraffin for three-dimensional printing forming as well as preparation method and application thereof

By using CT developable paraffin wax, a combination wax of solid paraffin, palm wax, natural resin and beeswax, and calcium sulfate dihydrate developing material, the problem of difficulty in reproducing the internal structure of the three-dimensional printing technology in the medical and dental fields has been solved, and individualization has been achieved. Customization and operation are simplified, reducing risk and cost, suitable for precision manufacturing in multiple industries.

CN118852884APending Publication Date: 2024-10-29XINQIAOTONG TECHNOLOGY (DALIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410914515.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing 3D printing technology is difficult to completely reproduce the internal structure of the target part in the medical and dental fields, which makes individual customization difficult, increases design and treatment risks, and is complex to operate, making it unsuitable for doctors and ordinary users with non-IT backgrounds.

Method used

A combination wax including solid paraffin, palm wax, natural resin and beeswax is used, calcium sulfate dihydrate developing material and pigment are added, and the developing material is melted by heating and evenly distributed to form CT developable paraffin wax, which can be used for three-dimensional printing and molding, simplifying operation and improve molding accuracy.

Benefits of technology

It achieves individual customization without design and treatment risks in 3D printing, simplifies the operation process, reduces costs, is suitable for precision manufacturing in medical, dental, construction, decoration, jewelry and other fields, and improves user participation and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852884A_ABST
    Figure CN118852884A_ABST
Patent Text Reader

Abstract

The invention discloses CT developable paraffin for three-dimensional printing forming, a preparation method and application. The CT developable paraffin mainly comprises combined wax A, a developing material C and pigment B, wherein the combined wax A comprises solid paraffin, palm wax, natural resin and beeswax, and the mass ratios of all the components in the combined wax A are as follows: 30 to 60 percent of solid paraffin, 10 to 20 percent of palm wax, 10 to 20 percent of natural resin and 20 to 30 percent of beeswax. The developing material C is one of calcium sulfate dihydrate, titanium dioxide and barium sulfate, and the addition amount of the developing material C is 1-30% of the mass of the combined wax A. And the pigment B is one of red oil, Sudan blue and Sudan yellow, and the addition amount of the pigment B is 0.01-1% of the mass of the combined wax A. The product is simple in preparation and use method and wide in applicable crowd, and the required shape is manufactured through direct operation on a model, so that the barrier and related cost of three-dimensional printing are greatly reduced. The product is wide in application range, and can be used in the aspects of building, decoration design, jewelry, mechanical product design and the like outside the medical and dental fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a paraffin composition, a preparation method and application of the composition. Background Art

[0002] With the development of 3D printing technology, 3D printing has gradually been applied to many fields such as aviation, mechanical manufacturing, design, medical treatment, and construction. 3D printing technology is a rapid manufacturing technology based on digital models of material stacking. This technology abandons traditional machine tools and molds, can greatly shorten the product development cycle, and can correspond to products with complex shapes. The biggest difference from traditional manufacturing is that 3D printing uses additive manufacturing, which effectively reduces the design and development time and cost of products. In addition, in the medical field, especially in the fields of dentistry, orthopedics, and regenerative medicine, it is possible to print complex-shaped organs of the human body, making personalized medicine possible.

[0003] However, the use of 3D printing technology requires advanced 3D molding software technology, and the relevant education and training time is relatively long. Even after mastering the operation of 3D molding software and other technologies, in actual clinical applications, the software operation time is long. Doctors without IT background and technology and doctors in grassroots hospitals find it difficult to quickly use related software in their busy work. This is also an important reason why 3D printing technology cannot be widely used in the medical industry.

[0004] In addition, the demand for individual customization in industries such as architecture, decoration, design, and jewelry is even greater. Since repeated modifications are required based on customer needs, simple software operations using symmetrical structures for three-dimensional molding are more difficult to implement or require a lot of time.

[0005] At present, the 3D printing technologies on the market are mainly divided into digital light processing (DLP), laser stereolithography (SLA), selective laser sintering (SLS) and melt lamination (FDM). Among them, the 3D printing technology based on digital light processing has the advantages of short molding time, not being restricted by complex 3D structures and individual customization, etc. However, it is difficult for optical molding technology to completely reproduce the internal structure of the target part, especially in medical and dental fields. It is easy to cause dead space, infection and other problems during surgery, which leads to the inability to achieve complete individual customization, increase the risk of design or treatment, and even cause reoperation, bringing unnecessary risks and losses to users. Summary of the invention

[0006] In order to make up for the deficiencies of the prior art, the purpose of the present invention is to provide an ideal CT developable paraffin for three-dimensional printing that is easy for ordinary technicians to master and can fully reproduce the internal structure of the target part without design and treatment risks.

[0007] The product to be protected by the present invention is a composition, which mainly includes: combined wax A, developing material C and pigment B. The combined wax A includes solid paraffin, palm wax, natural resin and beeswax, solid paraffin is the main component of the combined wax A, palm wax can improve the melting point and glossiness of solid paraffin and increase its hardness and inhibit flow, the role of natural resin is to increase the viscoelasticity of the combined wax A and lubricate the surface, improve the glossiness, and the role of beeswax is to increase the softness and glossiness of the combined wax A. The mass ratios of the components in the combined wax A are: solid paraffin 30-60%, palm wax 10-20%, natural resin 10-20%, beeswax 20-30%.

[0008] The composite wax obtained by solid paraffin wax, palm wax, natural resin and beeswax has good viscoelasticity, moderate hardness, softness and fluidity, is easy to process, and maintains a certain glossiness, and can be applied to three-dimensional printing molding technology, providing a new idea for industrial production. Before the present invention, people have not found that the composite wax can be effectively applied in three-dimensional printing molding technology.

[0009] The developing material C is one of calcium sulfate dihydrate, titanium dioxide and barium sulfate, and is used to obtain scanned images after CT scanning, and its addition amount is 1-30% of the mass of the combined wax A. The CT developing material C of the present invention can meet the following requirements: CT can be developed, can be evenly distributed in paraffin, and its CT value can be clearly distinguished from the model material and air.

[0010] Pigment B is red oil (molecular formula C 26 H 24 N40), Sudan blue (molecular formula C 22 H 18 N2O2), Sudan Yellow (molecular formula C 16 H 13 N3), the pigment is added mainly to make it more intuitive and beautiful, so that developers and users can clearly specify the parts that need to be processed or modified during design and communication. The added amount is 0.01-1% of the mass of the combined wax A.

[0011] The present invention also claims protection for a method for preparing the above-mentioned product, which specifically comprises the following steps:

[0012] S1. Weigh and mix solid paraffin, palm wax, natural resin and beeswax in the proportion to obtain a wax combination A, and then weigh the developer C and pigment B in the proportion;

[0013] S2. Add the wax combination A to the heating container and heat to a temperature of 40-120 ° C and maintain it at this temperature while stirring until it is completely melted;

[0014] S3. Then, the developer C is added to the molten wax combination A in step S2, and the heating is continued and maintained at a temperature of 40-120°C, and the developer C is stirred so that the developer C is evenly distributed in the wax combination A;

[0015] S4. As needed, add a color pigment in pigment B to the mixture in the hot melt state of step S3, continue heating and maintain the temperature at 40-120 ° C, while stirring to uniformly dissolve pigment B in the mixture of the combination wax A and the developer material C;

[0016] S5. Finally, the product is processed into the desired shape as needed.

[0017] The present invention also requests protection for the application of the above-mentioned product, that is, the above-mentioned CT developable paraffin wax can be widely used in precision manufacturing in multiple industries such as 3D printing, medical materials, construction and decoration materials, product design, and jewelry. Furthermore, medical materials include but are not limited to dental materials and bone model materials. Construction and decoration materials include but are not limited to building sand table models and interior decoration design models. Product design includes but is not limited to machine components and precision parts.

[0018] The present invention claims a method for using CT developable paraffin, comprising the following steps:

[0019] S1. The CT-developable paraffin is heated to soften and melt, and then the product is applied to the model or object; or the shaped product provided by the CT-developable paraffin is attached to make the user's desired shape, that is, the wax model;

[0020] S2. Scan the wax-up model using CT, convert the scanned data into DICOM format, start the 3D modeling software, and create a 3D model on the software;

[0021] S3. Edit the filter on the 3D modeling software, either automatically or manually;

[0022] S4. Generate the basic shape into STL format, input relevant parameters after determining the generated shape, and confirm;

[0023] S5. Generate a 3D model;

[0024] S6. Use Magic software to perform subsequent filter editing operations, modify the 3D model on the computer and add color;

[0025] S7. Send the 3D model to the customer for confirmation;

[0026] S8. Import the STL data into the 3D printer to print the final product.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] 1. The preparation and use methods of the product of the present invention are simple and applicable to a wide range of people. By directly operating on the model, the desired shape can be produced, thereby greatly reducing the barriers to three-dimensional printing and reducing the relevant costs of three-dimensional printing companies.

[0029] 2. The product of the present invention can be used by simple heating equipment such as an alcohol lamp, does not require special operating environment and conditions, and has a wide range of applications. It can be used in construction, decoration design, jewelry, mechanical product design, etc. in addition to the medical and dental fields.

[0030] 3. The product of the present invention combines raw materials in accordance with the standard requirements for medical devices, is non-toxic, harmless and has no side effects on the human body. In the medical field, compared with general three-dimensional scanners that can obtain images of internal structures, individual customized artificial organ materials can be closer to the real shape of the human body, reducing the risks of surgery or treatment.

[0031] 4. The present invention uses paraffin as the main component, which can be melted by heating and can be repeatedly operated without damaging the original model and mold, greatly improving the user's enthusiasm for participating in three-dimensional printing and the efficiency of three-dimensional printing.

[0032] 5. The product of the present invention can be reused, which not only reduces the consumption of raw materials but also reduces the cost of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a photograph of Application Example 1 in which the product of the present invention is applied to the affected area on a plaster model.

[0034] Figure 2 It is a CT image of the plaster model and the target object of Application Example 1.

[0035] Figure 3 This is a photo of the artificial bone printed in Application Example 1. DETAILED DESCRIPTION

[0036] In order to more clearly explain the purpose, technical solutions and advantages of the present invention, the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. It should be understood that the following description of the embodiments is intended to explain and illustrate the overall concept of the present invention, and should not be understood as limiting the present invention. In the specification and the drawings, the same or similar reference numerals refer to the same or similar parts or components. For the sake of clarity, the drawings are not necessarily drawn to scale, and some well-known parts and structures may be omitted in the drawings.

[0037] Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field. The wording "one" or "an" in the present invention does not exclude multiple. "Include" or "comprise" and other similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, but do not exclude other elements or objects. "Up", "down", "left", "right", "top" or "bottom" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0038] The basic composition properties of the paraffin mentioned in the examples of the present invention are shown in the following table:

[0039] Table 1 Analysis of properties of basic components of paraffin

[0040]

[0041] Example 1

[0042] (1) Preparation:

[0043] Take 60 grams of solid paraffin, 10 grams of palm wax, 10 grams of natural resin and 20 grams of beeswax, and mix them together to obtain composite wax A. Then weigh 3 grams of developer C, namely titanium dioxide, and 0.01 grams of pigment B, namely red oil. Add composite wax A to a conical flask, and heat it to 40°C with a heating stirrer and maintain it at this temperature until the composite wax A is completely melted. Then add developer C titanium dioxide to the molten composite wax A in the conical flask, continue to heat and maintain the temperature at 40°C with a heating stirrer, stir for 5 minutes until it is evenly distributed, and then add pigment B red oil to the molten mixture in the conical flask, continue to heat and maintain the temperature at 40°C, and stir for 2 minutes. Finally, process the product into a cylinder.

[0044] (2) Detection:

[0045] The obtained product was tested. The specific operation method was: using a CT (full name) produced by Toshiba Japan for scanning. The CT imaging conditions were set as follows: slice 0.5mm, resolution 512x512pxd, voltage 120kV. In a mold with an inner diameter of 30mm and an outer diameter of 40mm. After testing, the CT value of this product was 166Hu, the CT value change rate of the boundary was 244, and the dispersion of the developing material was 194Hu.

[0046] Example 2

[0047] (1) Preparation: This embodiment is basically the same as Embodiment 1, except that the developing material C is 15 g of titanium dioxide.

[0048] (2) Testing: The prepared product was tested in the same manner as in Example 1. The CT value of the product was found to be 266 Hu, the change rate of the CT value at the boundary was 342, and the dispersibility of the developing material was 598 Hu.

[0049] Example 3

[0050] (1) Preparation: Take 30 grams of solid paraffin, 20 grams of palm wax, 20 grams of natural resin and 30 grams of beeswax, and mix them together to obtain composite wax A. Then weigh 1.5 grams of developer C, i.e. barium sulfate, and 1 gram of pigment B, i.e. Sudan yellow. Add composite wax A to a conical flask, and heat it to 120°C with a heating stirrer and maintain it at this temperature until the composite wax A is completely melted. Then add developer C, i.e. barium sulfate, to the molten composite wax A in the conical flask, continue heating with a heating stirrer and maintain the temperature at 120°C, stir for 5 minutes until it is evenly distributed, and then add pigment B, i.e. Sudan yellow, to the molten mixture in the conical flask. Continue heating and maintain the temperature at 120°C and stir for 3 minutes. Finally, process the product into an amorphous body and package it in a box.

[0051] (2) Testing: The obtained product was tested in the same manner as in Example 1. The CT value of the product was 184Hu, the change rate of the CT value at the boundary was 239, and the dispersibility of the developing material was 386Hu.

[0052] Example 4

[0053] (1) Preparation: This embodiment is basically the same as Embodiment 3, except that the developing material C is 4 g of barium sulfate.

[0054] (2) Testing: The obtained product was tested in the same manner as in Example 1. The CT value of the product was 199 Hu, the change rate of the CT value at the boundary was 276, and the dispersibility of the developing material was 574 Hu.

[0055] Example 5

[0056] (1) Preparation: Take 45 grams of solid paraffin, 15 grams of palm wax, 15 grams of natural resin and 25 grams of beeswax, and mix them together to obtain composite wax A. Then weigh 6 grams of developing material C, namely calcium sulfate dihydrate, and 0.1 grams of pigment B, namely Sudan blue. Add composite wax A to a conical flask, and heat it to 120°C with a heating stirrer and maintain it at this temperature until the composite wax A is completely melted. Then add developing material C, namely calcium sulfate dihydrate, to the molten composite wax A in the conical flask, continue to heat and maintain the temperature at 120°C with a heating stirrer, stir for 5 minutes until it is evenly distributed, and then add pigment B, namely Sudan blue, to the molten mixture in the conical flask. Continue to heat and maintain the temperature at 120°C and stir for 3 minutes. Finally, process the product into a triangular prism.

[0057] (2) Testing: The obtained product was tested in the same manner as in Example 1. The CT value of the product was found to be 190 Hu, the change rate of the CT value at the boundary was 252, and the dispersibility of the developing material was 140 Hu.

[0058] Example 6

[0059] (1) Preparation: This embodiment is basically the same as Embodiment 3, except that the developing material C is 30 g of calcium sulfate dihydrate.

[0060] (2) Testing: The obtained product was tested in the same manner as in Example 1. The CT value of the product was 360 Hu, the change rate of the CT value at the boundary was 300, and the dispersibility of the developing material was 195 Hu.

[0061] Experiments have shown that the greater the rate of change of the CT value at the boundary, the clearer the boundary between the paraffin and the plaster can be developed, thereby accurately reconstructing the simulated contour.

[0062] The CT-developable paraffin wax of the present invention is prepared by the following method:

[0063] Heat the product of the present invention to soften and melt it, then apply the product of the present invention on the model or object; or use the shaped product provided by the product of the present invention to stick and attach to make the user's desired shape, i.e. wax model, then use CT (medical or industrial) to scan the wax model, and then convert the scan data into DICOM data. Start the 3D modeling software (Mimics), and perform the following operations on the software to make a 3D model. 1. Select [Import Images] to generate a Mimics Document from DICOM data. 2. Create a filter (Musk) for editing on the Mimics Document, and then draw a Profile Line on the CT image. 3. There are two ways to edit the filter: 1) Automatic editing: change the Thresholds value of the filter and submit it to generate. 2) Manual editing: apply it on the position of the paraffin to generate it. 4. Generate the basic shape in STL format. After determining the generated shape, enter the relevant parameters and click OK. 5. Generate a 3D model. 6. Use Magic software to perform subsequent filter editing operations, modify the 3D model on the computer and add color. 7. Send the 3D model to the customer for confirmation. 8. Import the STL data into the 3D printer and print the final product.

[0064] The application fields of the product of the present invention include but are not limited to 3D printing, medical materials, construction and decoration materials, product design, precision manufacturing of jewelry and other industries. Examples are as follows:

[0065] Application Example 1

[0066] Taking the filling of the patient's skull as an example

[0067] The CT DICOM data of the patient is processed by 3D shaping software and then input to a 3D printer to print out a plaster model of the patient's head. The doctor takes a triangular prism CT-developable paraffin similar in shape to the affected part, heats it with an alcohol lamp to soften it, and then places it on the corresponding affected part of the plaster model and applies the product of the present invention according to the shape of a normal person. Figure 1 The pink part indicated by the arrow was placed at room temperature for 30 minutes, and then the plaster model coated with the product of the present invention was subjected to CT scanning. The CT image of the target object after coating is as follows: Figure 2 The gray part pointed by the arrow converts the data into DICOM format data. Start the 3D modeling software (Mimics) and perform the following operations on the software to create a 3D model. 1. Select [ImportImages] to generate a Mimics Document from the DICOM data. 2. Create a filter (Musk) for the editing object on the Mimics Document, and then draw a Profile Line on the CT image. 3. Edit the filter, change the Thresholds value of the filter and submit it to generate. 4. Generate the basic shape in STL format. After confirming the generated shape, enter the relevant parameters and click OK to confirm. 5. Generate a 3D model. 6. Use Magic software to perform subsequent filter editing operations, and modify and add color to the 3D model on the computer. 7. Send the 3D model to the customer for confirmation. 8. Import the STL data into the 3D printer and print it into artificial bone, such as Figure 3 shown.

[0068] Application Example 2

[0069] In the production of dentures in the dental field, the dentist takes the boxed amorphous product of the present invention and places it on an alcohol lamp to heat it to soften it. Then, according to his own treatment plan and design, he applies the product on the pre-prepared plaster model until it meets his requirements, leaves it at room temperature for 30 minutes, and then performs CT scanning on the plaster model after applying the product of the present invention, and converts the data into DICOM data. Start the 3D modeling software (Mimics), and perform the following operations on the software to make a 3D model. 1. Select [Import Images] to generate a Mimics Document from DICOM data. 2. Create a filter (Musk) for the editing object on the Mimics Document, and then draw a Profile Line on the CT image. 3. Edit the filter, manually edit: apply it on the position of the paraffin to generate it. 4. Generate the basic shape in STL format. After determining the generated shape, enter the relevant parameters and click OK to confirm. 5. Generate a 3D model. 6. Use Magic software to perform subsequent filter editing operations, and operate, modify and add color to the 3D model on the computer. 7. Send the 3D model to the customer for confirmation. 8. Import the STL data into the 3D printer and print it into artificial teeth.

[0070] Application Example 3

[0071] In the production of sand table models in the field of architecture, at present, when developing houses, real estate companies have widely used the development of architectural model sand tables for publicity and introduction. However, when entrusting the processing of models, sometimes the sand table models need to be modified due to changes in actual conditions or needs. When making sand table models of buildings, you can first make basic designs and try to use modular designs. When displaying or explaining, prepare some cutting tools and heating equipment, heat the ends of the modified paraffin model and paste them on the sand table model to complete the modification and reconstruction of the model. Then use industrial CT to scan the model, convert it into DICOM data, perform three-dimensional reconstruction, extract the paraffin filling part, form an STL file, import it into a 3D printer, print it and fill it on the model to complete the production of the sand table model.

[0072] Application Example 4

[0073] Indoor decoration field. A 3D image of the indoor structure can be obtained through a 3D scanner or other equipment, and an indoor model can be printed for basic design. This product can be used to make basic shapes during design, or software can be used for interior decoration design, and a 3D printed design model can be delivered to the customer at the same time as the model, and the customer can make modifications or changes. After both parties reach a consensus on the design, the method disclosed in the present invention is used to obtain a 3D image using industrial CT scanning, and a 3D printer is used to print the interior decoration design model.

[0074] Application Example 5

[0075] Jewelry. Jewelry designers can use this product to carve wax plates according to design drawings, perform CT scanning to obtain three-dimensional image data, and after modification, they can output the production film to complete the product manufacturing.

[0076] Application Example 6

[0077] Machine component design can be designed according to drawings, filled or made using this product, completed through CT scanning, 3D printer prints samples, and then modified or designed before mass production.

[0078] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. CT-developable paraffin wax for three-dimensional printing, characterized in that: Comprising a combination of wax A, pigment B and developing material C; wherein, Combination wax A includes: Solid paraffin 30-60wt%; Palm wax 10-20wt%; Natural resin 10-20wt%; Beeswax 20-30wt%; The developing material C is one of calcium sulfate dihydrate, titanium dioxide, and barium sulfate; the added amount thereof is 1-30% of the mass of the combined wax A; The pigment B is added in an amount of 0.01-1% of the mass of the combined wax A.

2. The CT-developable paraffin according to claim 1, characterized in that: Pigment B is any one of red oil, Sudan blue or Sudan yellow.

3. The method for preparing CT-developable paraffin according to claim 1, characterized in that: The steps include: S1. The solid paraffin wax, palm wax, natural resin and beeswax were weighed and mixed together to obtain a wax combination A, and then the developer C and pigment B were weighed in the proportion; S2 is added to the heating container wax combination A, heated to a temperature of 40-120 ℃ and maintained at this temperature while stirring until all melted; S3 is then added to the molten wax combination A in step S2, the developer material C is heated and maintained at a temperature of 40-120 ℃, and stirred so that the developer material C is evenly distributed in the wax combination A; S4 as needed, to the heat-melted mixture in step S3 is added a color pigment in the pigment B, continue heating and maintain the temperature at 40-120 ℃, while stirring so that the pigment B is uniformly dissolved in the mixture of the wax combination A and the developer material C; S5. Finally, the product is processed into the desired shape as needed.

4. The preparation method according to claim 3, characterized in that The shape of the step S5 is a sheet, a triangular prism, a cylinder, a cuboid or an amorphous shape.

5. The use of the CT-developable paraffin wax according to claim 1, characterized in that: Including but not limited to 3D printing, medical materials, construction and decoration materials, product design, and precision manufacturing in the jewelry industry.

6. The use according to claim 5, characterized in that Medical materials include but are not limited to dental materials and bone model materials.

7. The use according to claim 5, characterized in that Construction and decoration materials include but are not limited to architectural sand table models and interior decoration design models.

8. The use according to claim 5, characterized in that The product design includes but is not limited to machine components and precision parts.

9. A method for using the CT-developable paraffin wax according to claim 1, characterized in that: The steps include: S1. The CT-developable paraffin is heated to soften and melt, and then the product is applied to the model or object; or the CT-developable paraffin provides a shaped product to be attached and pasted to produce the desired shape of the user, namely, a wax model; S2. Scan the wax-up using CT, convert the scan data into DICOM format, launch 3D modeling software, and create a 3D model in the software; S3. Edit filters in the 3D modeling software, either automatically or manually. S4. Generate the basic shape into STL format. After confirming the generated shape, enter the relevant parameters and confirm. S5. generating a 3D model; S6. Use Magic software to perform subsequent filter editing operations, modify the 3D model and add color on the computer; S7. Send the 3D model to the customer for confirmation; S8. Import the STL data into the 3D printer to print the final product.

10. The method according to claim 9, characterized in that The step S3 includes 1) automatic editing: changing the Thresholds value of the filter and submitting it to generate; 2) manual editing: applying it on the position of the paraffin to generate.