Ceramics, thermoelectric effect elements, electronic components and electronic devices
By adjusting the composition of PbSc0.5-xTa0.5+xO3-mPbMg0.5-yW0.5+yO3, the problem of insufficient thermoelectric effect of PMW ceramics under low electric field was solved, and a large thermoelectric effect was achieved under low electric field, which is suitable for cooling systems.
Patent Information
- Application Number
- CN202380021441.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing PMW ceramics exhibit relatively small thermoelectric effects under low electric fields, requiring high electric fields to show significant effects, which leads to complex electric field strength and control.
By adjusting the composition of PbSc0.5-xTa0.5+xO3-mPbMg0.5-yW0.5+yO3, especially by controlling the ranges of x, y, and m, it can exhibit a large thermoelectric effect under a low electric field, thereby reducing the threshold voltage and the transition temperature.
It achieves a large thermoelectric effect under low electric field, simplifies electric field control, is suitable for cooling systems, and exhibits excellent thermoelectric effect, especially in the temperature range below room temperature.
Smart Images

Figure CN118871405B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to ceramics. Background Technology
[0002] In recent years, novel solid-state cooling elements and systems utilizing the thermoelectric effect have attracted considerable attention as cooling components, and their research and development are extensive. Compared with existing cooling systems that use refrigerants that are greenhouse gases, these systems offer advantages such as not requiring refrigerants, high efficiency, and low power consumption. Furthermore, because they do not use compressors, they are quieter. To obtain excellent thermoelectric effects, materials are required that have a transition temperature within the desired temperature range and can be subjected to a large electric field. PbSc is such a material. 0.5 Ta 0.5 O3 (hereinafter, ceramics containing Pb, Sc, and Ta will also be referred to as "PST") (Patent Document 1, Non-Patent Documents 1-2), and PbMg 0.5 W 0.5 O3 (hereinafter, ceramics containing Pb, Mg, and W will also be referred to as "PMW") is known as a promising material. Non-Patent Document 3 mentions PbMg 0.5 W 0.5 O3 exhibits both large positive and negative thermoelectric effects.
[0003] Prior art literature
[0004] Patent documents
[0005] Patent Document 1: International Publication No. 2021 / 131142
[0006] Non-patent literature
[0007] Non-patent literature 1: Nature, volume 575, pp. 468-472 (2019)
[0008] Non-patent literature 2: Ferroelectrics, 184, 239 (1996)
[0009] Non-patent literature 3: Adv. Funct. Mater. 31, 2101176 (2021). Summary of the Invention
[0010] The problem the invention aims to solve
[0011] PMW is an antiferroelectric, which has the characteristic of transitioning to a ferroelectric by applying a voltage equal to or higher than a threshold voltage. Below this threshold voltage, the pyroelectric effect of PMW is very small, and once the threshold voltage is exceeded, the pyroelectric effect is exhibited in accordance with the magnitude of the applied voltage. That is, when PMW is used as a solid cooling element, it is necessary to apply a large voltage exceeding the threshold voltage of PMW, and the electric field strength required to exhibit the pyroelectric effect also becomes high.
[0012] An object of the present disclosure is to provide a ceramic that exhibits a large pyroelectric effect under a lower electric field than in the past. More specifically, the object is to provide a ceramic that exhibits a large pyroelectric effect under a low electric field as compared with conventional PMW.
[0013] Technical solutions for solving the problem
[0014] The present disclosure relates to a ceramic represented by formula (1),
[0015] (1-m)PbSc 0.5-x Ta 0.5+x O3-mPbMg 0.5-y W 0.5+y O3(1)
[0016] [In formula (1),
[0017] m satisfies 0.60≤m≤0.95,
[0018] when 0≤x and 0≤y, x≤0.1, y≤0.1 and 0≤x+y≤0.13 are satisfied,
[0019] when 0>x and 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied,
[0020] when 0≥x and 0>y, -0.1≤x, -0.1≤y and -0.13≤x+y<0 are satisfied,
[0021] when 0<x and 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.].
[0022] The present disclosure includes the following embodiments.
[0023] [1] A ceramic represented by formula (1),
[0024] (1-m)PbSc 0.5-x Ta 0.5+x O3-mPbMg 0.5-y W 0.5+y O3(1)
[0025] [In formula (1),
[0026] m satisfies 0.60≤m≤0.95,
[0027] Under the condition of 0≤x and 0≤y, x≤0.1, y≤0.1 and 0≤x+y≤0.13 are satisfied,
[0028] Under the condition of 0>x and 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied,
[0029] Under the condition of 0≥x and 0>y, -0.1≤x, -0.1≤y and -0.13≤x+y<0 are satisfied,
[0030] Under the condition of 0<x and 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.].
[0031] [2] The ceramic according to the above [1], wherein
[0032] In the formula,
[0033] Under the condition of 0≤x and 0≤y, 0≤x+y≤0.1 is satisfied,
[0034] Under the condition of 0≥x and 0>y, -0.1≤x+y<0 is satisfied.
[0035] [3] The ceramic according to the above [1] or [2], wherein
[0036] In the formula, x is 0 and y is 0.
[0037] [4] The ceramic according to any one of the above [1] to [3], wherein
[0038] In the formula, m satisfies 0.6≤m≤0.9.
[0039] [5] The ceramic according to any one of the above [1] to [4], wherein
[0040] The crystal structure of the ceramic has a perovskite structure.
[0041] [6] A thermoelectric element, in which noble metal electrodes and the ceramic according to any one of the above [1] to [5] are alternately laminated.
[0042] [7] The thermoelectric element according to the above [6], wherein
[0043] The noble metal electrode is formed of Pt.
[0044] [8] An electronic component configured to have the thermoelectric element according to the above [6] or [7].
[0045] [9] An electronic device configured to have a thermoelectric effect element as described in [6] or [7] above or an electronic component as described in [8] above.
[0046] Invention Effects
[0047] According to this disclosure, it is possible to provide a ceramic that exhibits a large thermoelectric effect under a low electric field. More specifically, it is possible to provide a ceramic that exhibits a larger thermoelectric effect under a low electric field compared to conventional PMWs. Attached Figure Description
[0048] Figure 1 The polarization-electric field intensity curve of the PMW at 15℃ is shown.
[0049] Figure 2 The polarization-electric field intensity curves of the sample within the scope of the present invention at -18°C are shown.
[0050] Figure 3 This is a schematic cross-sectional view of a thermoelectric effect element as one embodiment of this disclosure.
[0051] Figure 4 It is a diagram used to illustrate the measurement sequence of the thermoelectric effect.
[0052] Figure 5 The polarization-electric field intensity curve of PMW sample number 1 at 15°C is shown.
[0053] Figure 6 The relationship between the thermoelectric effect and electric field strength of PMW sample number 1 at 15°C is shown.
[0054] Figure 7 The relationship between the thermoelectric effect and temperature is shown for the PMW sample number 1 under an electric field strength of 20 MV / m.
[0055] Figure 8 The relationship between the thermoelectric effect and temperature is shown for PST sample number 2 under an electric field strength of 15 MV / m.
[0056] Figure 9 The relationship between the thermoelectric effect and temperature is shown for PST sample number 2 and sample number 6 under an electric field strength of 15 MV / m.
[0057] Figure 10 It is a graph showing the results of characteristic tests for various x and y compositions. Detailed Implementation
[0058] Hereinafter, the ceramic of the present disclosure and the thermoelectric effect element using the ceramic will be described in detail with reference to the accompanying drawings. However, the shape, arrangement, and the like of the thermoelectric effect element and each constituent element of the present embodiment are not limited to the examples shown in the drawings.
[0059] [Ceramic]
[0060] The ceramic according to one embodiment of the present disclosure contains Pb, Sc, Ta, Mg and W as main components. The above ceramic is a composite oxide containing Pb, Sc, Ta, Mg and W,
[0061] The content ratio of Pb is substantially equal to the total content ratio of Sc, Ta, Mg and W,
[0062] When the content ratio of Sc is set to "0.5-x", the content ratio of Ta is "0.5+x", and when the content ratio of Mg is set to "0.5-y", the content ratio of W is "0.5+y",
[0063] Regarding the ranges of x and y,
[0064] When 0≤x and 0≤y, x≤0.1, y≤0.1 and 0≤x+y≤0.13 are satisfied,
[0065] When 0>x and 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied,
[0066] When 0≥x and 0>y, -0.1≤x, -0.1≤y and -0.13≤x+y<0 are satisfied,
[0067] When 0<x and 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied,
[0068] When the total content ratio of Mg and W is set to "m", the total content ratio of Sc and Ta is "1-m", and the range of m is 0.60≤m≤0.95. In addition, all the above ratios are molar ratios. By setting the composition within the above range, a large thermoelectric effect can be obtained under a low electric field.
[0069] In addition, the aforementioned expression that "the content ratio of Pb is substantially equal to the total content ratio of Sc, Ta, Mg and W" is not limited to the case where the content ratio of Pb is completely equal to the total content ratio of Sc, Ta, Mg and W. That is, the expression that "the content ratio of Pb is substantially equal to the total content ratio of Sc, Ta, Mg and W" also includes cases where the difference between the content ratio of Pb and the total content ratio of Sc, Ta, Mg and W is, for example, within 3% in terms of molar ratio.
[0070] Regarding the composition of the ceramics disclosed herein, for example, it can be analyzed and determined by means of high-frequency inductively coupled plasma optical emission spectrometry, fluorescence X-ray analysis, etc.
[0071] The thermoelectric effect is an endothermic / exothermic phenomenon caused by the change in entropy of electric dipole moments within a substance, resulting from a change in the electric field, causing them to become uniform or disordered. In this invention, the performance index of the thermoelectric effect can also be the adiabatic temperature change (ΔT). That is, a "large thermoelectric effect" can also mean a large adiabatic temperature change (ΔT). In this invention, a larger adiabatic temperature change (ΔT) is preferred.
[0072] The adiabatic temperature change ΔT refers to the temperature change of a ceramic caused by applying an electric field to the ceramic and / or removing the electric field applied to the ceramic. Specifically, it can be the difference between the temperature of the ceramic before the electric field is applied and the temperature of the ceramic immediately after the electric field is applied, or it can be the difference between the temperature of the ceramic before the electric field is removed and the temperature of the ceramic immediately after the electric field is removed.
[0073] Generally, the greater the electric field strength applied to the ceramic, the greater the adiabatic temperature change ΔT. Furthermore, the adiabatic temperature change ΔT tends to be greater the closer the ceramic temperature is to the antiferroelectric transition temperature (or ferroelectric transition temperature) when the electric field is applied. For example, as the ceramic temperature falls below the transition temperature, the thermoelectric effect decreases sharply. Specifically, for conventional PMW ceramics with a transition temperature of approximately 20–30°C, the thermoelectric effect tends to decrease significantly when the ceramic temperature is below 0°C.
[0074] In another manner, the aforementioned ceramic can also be a ceramic represented by formula (1).
[0075] (1-m)PbSc 0.5-x Ta 0.5+x O3-mPbMg 0.5-y W 0.5+y O3(1)
[0076] In equation (1),
[0077] m satisfies 0.60 ≤ m ≤ 0.95.
[0078] Given 0 ≤ x and 0 ≤ y, the following conditions must be met: x ≤ 0.1, y ≤ 0.1, and 0 ≤ x + y ≤ 0.13.
[0079] In the case that 0 > x and 0 ≤ y, the following conditions must be met: -0.1 ≤ x < 0 and 0 ≤ y ≤ 0.1.
[0080] In the case of 0≥x and 0>y, -0.1≤x, -0.1≤y and -0.13≤x+y<0 are satisfied,
[0081] In the case of 0<x and 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.].
[0082] By setting x, y and m to the above ranges, a large thermoelectric effect can be obtained under a low electric field (for example, 0.8 K or more when an electric field strength of 8 MV / m is applied).
[0083] The present disclosure is not limited by any theory, but the mechanism by which the above-described effects can be obtained is considered to be as follows.
[0084] Examples of substances exhibiting a large thermoelectric effect include PMW which exhibits antiferroelectricity and PbSc which exhibits ferroelectricity 0.5 Ta 0.5 O3 (hereinafter, the ceramic containing Pb, Sc and Ta is also referred to as "PST"). PMW and PST respectively exhibit antiferroelectricity and ferroelectricity which have large latent heat at the time of transition due to the arrangement of cations at the B site (Mg and W for PMW, and Sc and Ta for PST).
[0085] In the case of PMW, a negative thermoelectric effect derived from its antiferroelectricity (heat absorption when an electric field is applied, heat generation when the electric field is removed) is exhibited below the phase transition temperature, and a large positive thermoelectric effect (heat generation when an electric field is applied, heat absorption when the electric field is removed) is exhibited near the transition temperature. That is, the sign of the thermoelectric effect is reversed depending on the temperature. As the thermoelectric effect used in practical applications, either a positive thermoelectric effect or a negative thermoelectric effect may be used. In the case of PMW, in order to obtain a large negative thermoelectric effect, a large electric field strength of 10 MV / m or more is required, and if it is less than 10 MV / m, only a very small thermoelectric effect is exhibited.
[0086] In general, it is known that the larger the difference in ionic radius between the two cations at the B site, the easier the arrangement. Compared with PST, PMW has a larger difference in ionic radius between Mg and W, so the B site is easy to be arranged. Unlike PST, PMW has the feature that the ions at the B site are arranged even without long-time heat treatment. In the present disclosure, the threshold voltage of the antiferroelectric is successfully reduced by adding PST to PMW. It is considered that this is because the arrangement at the B site of PMW is moderately lowered.
[0087] The so-called threshold voltage is as Figure 1As shown, this represents a voltage at which the polarization increases dramatically (approximately 18 MV / m). Below the threshold voltage, the polarizations cancel each other out; above the threshold voltage, the polarizations begin to align in the direction of the electric field. Under a stronger electric field, similar to a typical ferroelectric, the polarizations align entirely in one direction. That is, an antiferroelectric can be induced to have the same polarization as a ferroelectric by applying a voltage above the threshold voltage. Below the threshold voltage, the antiferroelectric's polarizations cancel each other out (…). Figure 1 The state of A in the equation (therefore, no thermoelectric effect is shown; if the threshold voltage is exceeded, the polarization becomes uniform) Figure 1 (The state of B in the voltage), thus showing a positive or negative thermoelectric effect depending on the magnitude of the voltage.
[0088] like Figure 2 As shown, with the ceramic of this disclosure, the threshold voltage decreases. Therefore, the ceramic of this disclosure exhibits a thermoelectric effect even under low electric fields. Furthermore, for ferroelectrics, once an electric field is applied, they become in a state with residual polarization (called remanent polarization), and correspondingly, the entropy change when the electric field is applied and when it is removed is smaller, resulting in a loss of thermoelectric effect. On the other hand, for antiferroelectrics, if the electric field is removed, the polarization completely returns to zero, thus no loss of thermoelectric effect occurs.
[0089] Furthermore, in this invention, by adding PST to the PMW, not only is the threshold voltage of the antiferroelectric material successfully reduced, but the transition temperature of the PMW is also successfully lowered to below room temperature. In other words, compared to conventional PMWs, the ceramic of this disclosure exhibits excellent thermoelectric effects even below 0°C (e.g., -15°C).
[0090] Furthermore, in this invention, it is possible to prevent the reversal of the positive and negative thermoelectric effects under relatively low electric field strengths (above 8 MV / m) within the actual operating temperature range (e.g., -20 to 0°C). Therefore, compared to conventional PMWs, the controllability of the thermoelectric effect of the ceramic disclosed herein is improved, and complex control is not required when using the ceramic disclosed herein as a cooling system.
[0091] In one approach, regarding the range of x and y,
[0092] Given 0 ≤ x and 0 ≤ y, the following conditions must be met: x ≤ 0.1, y ≤ 0.1, and 0 ≤ x + y ≤ 0.12.
[0093] In the case that 0 > x and 0 ≤ y, the following conditions must be met: -0.1 ≤ x < 0 and 0 ≤ y ≤ 0.1.
[0094] When 0 ≥ x and 0 > y, the following conditions must be met: -0.1 ≤ x, -0.1 ≤ y, and -0.12 ≤ x + y < 0.
[0095] In the case of 0<x, 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.
[0096] In one embodiment, regarding the ranges of x and y,
[0097] In the case of 0≤x, 0≤y, x≤0.1, y≤0.1 and 0≤x+y≤0.11 are satisfied,
[0098] In the case of 0>x, 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied,
[0099] In the case of 0≥x, 0>y, -0.1≤x, -0.1≤y and -0.11≤x+y<0 are satisfied,
[0100] In the case of 0<x, 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.
[0101] In one embodiment, regarding the ranges of x and y,
[0102] In the case of 0≤x, 0≤y, 0≤x+y≤0.1 is satisfied,
[0103] In the case of 0>x, 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied,
[0104] In the case of 0≥x, 0>y, -0.1≤x+y<0 is satisfied,
[0105] In the case of 0<x, 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.
[0106] In one embodiment, regarding the ranges of x and y,
[0107] In the case of 0≤x, 0≤y, 0≤x+y≤0.08 is satisfied,
[0108] In the case of 0>x, 0≤y, -0.08≤x<0 and 0≤y≤0.08 are satisfied,
[0109] In the case of 0≥x, 0>y, -0.08≤x+y<0 is satisfied,
[0110] In the case of 0<x, 0>y, 0<x≤0.08 and -0.08≤y<0 are satisfied.
[0111] In one embodiment, regarding the ranges of x and y,
[0112] In the case of 0≤x, 0≤y, 0≤x≤0.05 and 0≤y≤0.05 are satisfied,
[0113] Under the condition of 0>x and 0≤y, -0.05≤x<0 and 0≤y≤0.05 are satisfied,
[0114] Under the condition of 0≥x and 0>y, -0.05≤x<0 and -0.05≤y<0 are satisfied,
[0115] Under the condition of 0<x and 0>y, 0<x≤0.05 and -0.05≤y<0 are satisfied.
[0116] In another embodiment, regarding the ranges of x and y,
[0117] Under the condition of 0≤x and 0≤y, 0≤x+y≤0.05 is satisfied,
[0118] Under the condition of 0>x and 0≤y, -0.05≤x<0 and 0≤y≤0.05 are satisfied,
[0119] Under the condition of 0≥x and 0>y, -0.05≤x+y<0 is satisfied,
[0120] Under the condition of 0<x and 0>y, 0<x≤0.05 and -0.05≤y<0 are satisfied.
[0121] In one embodiment, the ranges of x and y may also be ranges determined by arbitrarily combining the x and y ranges under the above-listed "condition of 0≤x and 0≤y", "condition of 0>x and 0≤y", "condition of 0≥x and 0>y", and "condition of 0<x and 0>y".
[0122] In a preferred embodiment, the aforementioned x and y are 0. That is, the formula represented by (1-m)PbSc 0.5-x Ta 0.5+x O3-mPbMg 0.5-y W 0.5+y O3 becomes (1-m)PbSc 0.5 Ta 0.5 O3-mPbMg 0.5 W 0.5 O3.
[0123] In one embodiment, regarding m, 0.60<m≤0.95 is also acceptable.
[0124] From the viewpoint of enhancing the thermoelectric effect under a low electric field, the aforementioned range of m is preferably 0.60≤m≤0.90, more preferably 0.70≤m≤0.90, and further preferably 0.70≤m≤0.80.
[0125] From the viewpoint of improving the thermoelectric effect at low temperatures, the range of m is preferably 0.60≤m≤0.90, more preferably 0.65≤m≤0.90, and even more preferably 0.65≤m≤0.85.
[0126] From the perspective of obtaining a negative thermoelectric effect, the range of m mentioned above can also be 0.90≤m≤0.95.
[0127] From the perspective of obtaining a positive thermoelectric effect, the range of m mentioned above can also be 0.60≤m≤0.80.
[0128] One embodiment of the present invention relates to a ceramic whose crystal structure can also be perovskite. The term "ceramic with a perovskite structure" means not only ceramics having a "perovskite-type crystal structure," but also ceramics having a "perovskite-like crystal structure." For example, a ceramic with a perovskite structure can also be a ceramic with a crystal structure that can be identified as perovskite by those skilled in the art of ceramics in X-ray diffraction.
[0129] Thermoelectric element
[0130] The thermoelectric effect element disclosed herein has a laminate in which electrode layers and ceramic layers with ceramic as the main component are alternately stacked.
[0131] like Figure 3 As shown, a thermoelectric element 1 according to one embodiment of this disclosure has a laminate 6 in which electrode layers 2a and 2b (hereinafter, also collectively referred to as "electrode layers 2") and a ceramic layer 4 are alternately stacked, and external electrodes 8a and 8b (hereinafter, also collectively referred to as "external electrodes 8") connected to the electrode layers 2. The electrode layers 2a and 2b are electrically connected to the external electrodes 8a and 8b disposed on the end faces of the laminate 6, respectively. When a voltage is applied from the external electrodes 8a and 8b, an electric field is formed between the electrode layers 2a and 2b. Due to this electric field, the ceramic layer 4 heats up due to the thermoelectric effect. Furthermore, when the voltage is removed, the electric field disappears, and as a result, the ceramic layer 4 absorbs heat due to the thermoelectric effect.
[0132] The aforementioned electrode layer 2 is the so-called internal electrode. In addition to providing an electric field to the ceramic layer 4, the electrode layer 2 can also transfer heat between the ceramic layer 4 and the outside.
[0133] The aforementioned electrode layer may also be an electrode layer whose main component is a noble metal. Here, the term "main component is a noble metal" in the above-mentioned electrode layer means that the electrode layer is composed of 80% or more of noble metal by mass. For example, it means that the electrode layer is composed of 95% or more of noble metal by mass, more preferably 98% or more of noble metal by mass, even more preferably 99% or more of noble metal by mass, even more preferably 99.5% or more of noble metal by mass, and particularly preferably 99.9% or more of noble metal by mass.
[0134] In this specification, the term "noble metal" can refer to, for example, Au, Ag, Pt, or Pd. From the viewpoint of improving the thermoelectric effect at low temperatures, the main component of the electrode layer used in this disclosure can be Pt or Pd. That is, it can be a Pt electrode layer or a Pd electrode layer. However, from the viewpoint of improving chemical durability and / or cost, the aforementioned noble metal electrode layer can also be an alloy (e.g., Ag-Pd alloy, etc.) or mixture of Pt and / or Pd with other elements (e.g., Ag, Pd, Rh, Au, etc.). Even if the aforementioned Pt electrode layer or Pd electrode layer is composed of these alloys or mixtures, the same effect can be obtained. In addition, other elements that may be mixed in as impurities, especially unavoidable elements (e.g., Fe, Al2O3, etc.), can also be included. In this case, the same effect can also be obtained.
[0135] The thickness of the electrode layer 2 is preferably 0.2 μm or more and 10 μm or less, more preferably 1.0 μm or more and 5.0 μm or less, for example, it can be 2.0 μm or more and 5.0 μm or less, or 2.0 μm or more and 4.0 μm or less. By setting the thickness of the electrode layer to 0.5 μm or more, the resistance of the electrode layer can be reduced, and the heat transfer efficiency can be improved. Furthermore, by setting the thickness of the electrode layer to 10 μm or less, the thickness of the ceramic layer can be increased (and thus, the volume of the ceramic layer can be increased), which can further increase the heat transferred by thermoelectric effect as a whole element. In addition, the element can be further reduced in size.
[0136] The ceramic layer 4 mentioned above can use one type of ceramic as the main component, or it can use two or more types of ceramic as the main component.
[0137] Here, the phrase "using ceramic as the main component" in the aforementioned ceramic layer means that the ceramic layer is substantially composed of the desired ceramic. For example, it means that 90% or more by mass of the ceramic layer is the desired ceramic, more preferably 95% or more by mass, even more preferably 98% or more by mass, even more preferably 99% or more by mass, and particularly preferably 99.5% or more by mass. Other components may include crystal phases with structures different from perovskite structures, such as pyrochlore structures, and other elements mixed in as impurities, especially unavoidable elements (e.g., Zr, C, etc.).
[0138] The composition of the ceramic layer 4 can be determined using high-frequency inductively coupled plasma optical emission spectroscopy (ICP-OES) and fluorescence X-ray diffraction (XRD). Furthermore, the structure of the ceramic layer 4 can be determined using powder X-ray diffraction.
[0139] The thickness of the ceramic layer 4 is preferably 5 μm or more and 100 μm or less, more preferably 5 μm or more and 50 μm or less, even more preferably 10 μm or more and 50 μm or less, even more preferably 20 μm or more and 50 μm or less, and particularly preferably 20 μm or more and 40 μm or less. By increasing the thickness of the ceramic layer, the heat that the component can handle can be increased. By decreasing the thickness of the ceramic layer, a higher ΔT can be obtained, and furthermore, the withstand voltage can be improved.
[0140] The voltage withstand capability of the ceramic layer 4 is preferably 15 MV / m or higher, more preferably 20 MV / m or higher, and even more preferably 25 MV / m or higher. By increasing the voltage withstand capability of the ceramic layer, a larger voltage (electric field) can be applied, resulting in a larger ΔT.
[0141] The materials used to form the pair of external electrodes 8a and 8b are not particularly limited, and Ag, Cu, Pt, Ni, Al, Pd, Au, or alloys thereof (e.g., Ag-Pd, etc.) can be used. The electrodes can be made of these metals and glass, or they can be made of these metals and resin. Among these, Ag is particularly preferred.
[0142] The aforementioned thermoelectric effect element 1 has electrode layers 2 and ceramic layers 4 alternately stacked. However, in the thermoelectric effect element disclosed herein, the number of electrode layers and ceramic layers stacked is not particularly limited. Furthermore, the internal electrodes may not all be connected to the external electrodes. Depending on the need to alleviate stress caused by heat transfer, piezoelectricity, electrostriction, etc., internal electrodes that are not connected to the external electrodes may also be included.
[0143] In the aforementioned thermoelectric element 1, the internal electrode and the ceramic layer are substantially in contact across the entire surface. However, the thermoelectric element of this disclosure is not limited to this structure; any structure capable of applying a voltage (electric field) to the ceramic layer is not particularly limited. Furthermore, while the thermoelectric element 1 is a cuboid block shape, the shape of the thermoelectric element of this disclosure is not limited to this. For example, it can be cylindrical, sheet-like, and may also have irregularities or through holes. Additionally, the internal electrode may be exposed on the surface to facilitate heat transfer and heat exchange with the outside.
[0144] The ceramic and thermoelectric effect element of this embodiment described above are manufactured, for example, as follows.
[0145] High-purity lead oxide (Pb3O4), tantalum oxide (Ta2O5), scandium oxide (Sc2O3), magnesium carbonate (MgCO3), and tungsten oxide (WO3) are weighed as raw materials to achieve the desired composition ratio after calcination. The above raw materials are then pulverized and mixed with partially stabilized zirconia (PSZ) balls, pure water, and a dispersant using a ball mill. The pulverized and mixed slurry is then dried, granulated, and calcined, for example, at 800°C to 900°C in atmospheric conditions. The resulting calcined powder is mixed with PSZ balls, ethanol, toluene, and a dispersant, and pulverized. Next, a dissolved binder solution is added to the pulverized powder and mixed to prepare a slurry for sheet forming. The prepared slurry is formed into a sheet on a support and Pt electrode paste is printed on it. Printed and unprinted sheets are laminated into a desired structure, then pressed under 100 MPa to 200 MPa and cut to produce raw green chips. The green chips are then heat-treated in atmosphere at 500°C to 600°C to remove the binder. Next, using a sealed crucible, for example made of alumina, the removed green chip is fired together with PbZrO3 powder to create a Pb atmosphere at 800°C to 1400°C. Then, the end faces of the green chip are sanded, external electrode paste is applied, and it is sintered at a given temperature to obtain... Figure 3 The thermoelectric effect element shown.
[0146] The thermoelectric effect element disclosed herein exhibits excellent thermoelectric effect and can therefore be used as a thermal management element, particularly a cooling element (including cooling pump elements / heat pump elements of air conditioning units such as air conditioners, refrigerators, and freezers).
[0147] In addition, this disclosure also provides electronic components configured to have thermoelectric effect elements of this disclosure and electronic devices configured to have thermoelectric effect elements or electronic components of this disclosure.
[0148] As for electronic components, there are no particular limitations, but examples include: electronic components used in air conditioners, refrigerators, or freezers, or electronic components used in air conditioners for electric vehicles or hybrid vehicles (e.g., batteries); integrated circuits (ICs) such as central processing units (CPUs), hard disks (HDDs), power management ICs (PMICs), power amplifiers (PAs), transceiver ICs, and voltage regulators (VRs); light-emitting elements such as light-emitting diodes (LEDs), incandescent lamps, and semiconductor lasers; field-effect transistors (FETs); and other components, such as lithium-ion batteries, substrates, heat sinks, and housings, which are commonly used in electronic devices.
[0149] As an electronic device, there are no particular limitations; examples include air conditioners, refrigerators or freezers, air conditioners used as heat pumps, air conditioners for electric or hybrid vehicles, portable phones, smartphones, personal computers (PCs), tablet terminals, hard disk drives, data servers, and other small electronic devices.
[0150] The thermoelectric effect element disclosed herein can be used as a thermal management system (or temperature management system) to manage the heat (temperature) of the aforementioned electronic components and electronic devices. For example, a cooling system for cooling the aforementioned electronic components and electronic devices can be cited as an example of a thermal management system.
[0151] Example
[0152] <Fabrication of Thermoelectric Elements>
[0153] High-purity lead oxide (Pb3O4), tantalum oxide (Ta2O5), scandium oxide (Sc2O3), magnesium carbonate (MgCO3), and tungsten oxide (WO3) were prepared as raw materials. These raw materials were weighed to achieve the given composition ratios shown in Tables 1-4 after calcination, and then pulverized and mixed with partially stabilized zirconia (PSZ) balls (2 mm in diameter), pure water, and a dispersant using a ball mill for 16 hours. The pulverized and mixed slurry was then dried and granulated using a hot plate, and subsequently calcined at 850°C in atmospheric conditions for 2 hours.
[0154] The obtained calcined powder was mixed with 5 mm diameter PSZ balls, ethanol, toluene, and a dispersant for 16 hours and then pulverized. Next, a dissolved binder solution was added to the pulverized powder, and the mixture was mixed for 4 hours to prepare a slurry for sheet forming. The prepared slurry was formed into sheets on PET film using a doctor blade to a thickness corresponding to the given ceramic layer thickness, and then cut into strips. Platinum internal electrode paste was then screen-printed onto the strips. Furthermore, the sheet thickness of the fabricated multilayer element was controlled by varying the gap of the doctor blade used during sheet forming.
[0155] A predetermined number of sheets were stacked, one with platinum internal electrode paste printed on it and the other without. These sheets were then pressed together under 150 MPa and cut to produce unprocessed small pieces. The unprocessed small pieces were then heat-treated at 550°C for 24 hours in atmosphere to remove the binder. Next, the unprocessed small pieces, along with PbZrO3 powder for creating a Pb atmosphere, were sealed in a bauxite crucible and fired at 900–1300°C for 4 hours. Samples within the scope of this invention can be fully fired at temperatures of 900–1250°C. Sample No. 1, shown in Table 1 as a comparative example, was fired at a high temperature of 1400°C and then heat-treated at 1000°C for 1000 hours.
[0156] Then, the end face of the small piece was sanded with sandpaper, and Ag external electrode paste was applied. It was then welded at 750°C to obtain the desired result. Figure 3 The thermoelectric effect element shown.
[0157] For a device with a ceramic layer thickness of 40 μm, the resulting device size is approximately L10.2 mm × W7.2 mm × T0.88. Furthermore, there are 19 ceramic layers sandwiched between internal electrode layers, with an electrode area of 49 mm². 2 / layer, total electrode area 49mm² 2 ×19 layers. Furthermore, after grinding the end faces of the components, the thickness of the ceramic layers in the components obtained above was confirmed using a scanning electron microscope.
[0158] <Evaluation>
[0159] (composition)
[0160] The ceramic composition of the obtained components was confirmed using high-frequency inductively coupled plasma optical emission spectroscopy and fluorescence X-ray diffraction.
[0161] (Crystal Structure)
[0162] To evaluate the crystal structure of the obtained components, powder X-ray diffraction was performed. A component was randomly selected from each batch, pulverized in a mortar, and X-ray diffraction patterns were obtained. Based on the obtained X-ray diffraction patterns, it was confirmed whether the ceramic crystal structure was perovskite. Furthermore, the presence and proportion of impurity phases (mainly pyrochlore phase) were estimated based on the intensity ratio. A perovskite structure presence ratio of 0.95 or higher was considered to indicate that the main component possessed a perovskite structure, while a perovskite structure presence ratio of less than 0.95 was considered to indicate the presence of heterogeneous phases.
[0163] (Thermoelectric effect)
[0164] A very fine K thermocouple with a diameter of 50 μm was adhered to the center of the element surface using Kapton tape, and the temperature was monitored at all times. Leads for applying voltage were attached to both ends of the external electrode using Ag paste, and a voltage was applied using a high voltage generating device.
[0165] By pressing Figure 4 The thermoelectric effect was evaluated by applying voltage to the sample in the sequence shown in graph (a). Specifically, a voltage was first applied to the sample and held as is; then the applied voltage was removed, and this process was repeated, and the change in thermoelectric effect was measured. When voltage was applied to the ferroelectric material in this sequence, the sample temperature rose simultaneously with the voltage application; during the holding phase, heat gradually diffused, and the sample temperature dropped to the same level as before the voltage application; during the removal phase, the sample temperature decreased simultaneously with the removal; and during the holding phase, the sample temperature gradually rose back to its original temperature (see reference). Figure 4 (b) This is because the ferroelectric domains become uniform or disordered when a voltage is applied and removed, resulting in an endothermic / exothermic effect (thermoelectric effect) through entropy changes.
[0166] On the other hand, in accordance with Figure 4 The sequence shown in graph (a) applies a voltage to the antiferroelectric material, such as... Figure 4 As shown in (c), in a specific temperature region, a thermoelectric effect opposite to that of ferroelectric materials is shown, that is, a negative thermoelectric effect is shown where the temperature decreases (endothermic) when a voltage is applied and increases (exothermic) when the voltage is removed.
[0167] Regarding the adiabatic temperature change ΔT, in this embodiment, a given voltage was applied, maintained for 50 seconds, and the temperature was measured. Then, the voltage was removed, and the state without voltage application was maintained for 50 seconds, and the temperature was measured again. This sequence was repeated three times. Throughout the voltage application and removal sequences, the element temperature was measured, and the adiabatic temperature change ΔT was calculated based on this temperature change. Furthermore, samples with absolute values of adiabatic temperature change ΔT exceeding 0.8 K and 1.5 K respectively when applied with electric fields of 8 MV / m and 15 MV / m at -15°C were subjected to a Go-class judgment. The results are shown in Tables 1 to 4.
[0168] The evaluation results described above are shown below. Additionally, samples marked with "※" in the table are comparative examples, while the other samples are exemplary examples.
[0169] [Table 1]
[0170]
[0171] [Table 2]
[0172]
[0173] [Table 3]
[0174]
[0175] [Table 4]
[0176]
[0177] The ferroelectric properties of the previous PMW, as shown in sample number 1, are illustrated below. Figure 5 The thermoelectric effect is shown in Figure 6 as well as Figure 7 .like Figure 5 As shown, conventional PMW exhibits the characteristic double hysteresis for antiferroelectrics, namely, as the electric field strength increases, the polarization increases sharply from the threshold voltage (approximately 15 MV / m), and saturates at higher electric field strengths. The threshold voltage is approximately 15 MV / m at 15 °C, but as the temperature decreases, the threshold voltage increases, requiring a larger electric field.
[0178] Figure 6 The figure shows the adiabatic temperature change ΔT measured at 15°C while changing the electric field strength. Figure 7 The diagram shows the adiabatic temperature change ΔT measured while the electric field strength was fixed at 20 MV / m and the temperature was varied. For example... Figure 6 As shown, a negative thermoelectric effect was obtained at 15°C, characterized by heat absorption when an electric field was applied and heat generation when the electric field was removed. However, considering the relationship between the adiabatic temperature change ΔT and the electric field strength, it can be confirmed that the thermoelectric effect is almost negligible at low electric fields, and gradually increases from near the threshold voltage. In other words, while a negative thermoelectric effect can be obtained with a PMW, a sufficient thermoelectric effect is not achieved without a large electric field of 12 MV / m or higher. Therefore, with a PMW, not only is a high electric field strength required, but it is also difficult to control the thermoelectric effect by changing the electric field strength.
[0179] like Figure 7As shown, when focusing on the temperature dependence of the adiabatic temperature change ΔT, it can be confirmed that at temperatures below 0°C, the obtainable electrothermal effect is very small even under an electric field strength of 20 MV / m. Regarding PMW, since its transition temperature is around 20°C, the sign of the adiabatic temperature change ΔT changes at 20°C near the transition temperature, and a positive electrothermal effect that generates heat upon voltage application and absorbs heat upon voltage removal can be obtained above 20°C. As such, in the case of an antiferroelectric, the sign of the electrothermal effect reverses in the temperature region spanning the transition temperature, making it extremely difficult to control. Therefore, simply lowering the transition temperature of an antiferroelectric may cause the problem that the sign of the electrothermal effect reverses within the assumed operating temperature range.
[0180] In Figure 8 the electrothermal effect of PST shown in conventionally known Sample No. 2 is presented. Unlike PMW, PST yields a positive electrothermal effect over the entire temperature range, and the adiabatic temperature change ΔT is maximized near the transition temperature of 20°C, providing a very excellent electrothermal effect. However, below 0°C, this effect drops sharply, and a sufficient effect cannot be obtained at low temperatures.
[0181] Table 1 shows the characteristic test results of the samples produced as described above. Specifically, Table 1 shows the electrothermal effect of samples in which the values of x and y in Formula (1) are fixed at 0 and m is changed to various values. As a result of XRD measurement performed on the samples having the compositions shown in Table 1, all of the main components have the desired perovskite structure with few heterogeneous phases.
[0182] The conventionally known PMW shown in Sample No. 1 and PST shown in Sample No. 2 have low electrothermal effects at -15°C, with an adiabatic temperature change of less than 1.5K. On the other hand, among the samples with compositions within the scope of the present invention, the absolute values of the adiabatic temperature change are 0.8K and 1.5K or more respectively when electric fields of 8 MV / m and 15 MV / m are applied.
[0183] Furthermore, for samples with m in the range of 0.6≤m≤0.8, a positive electrothermal effect is exhibited in the range of -20°C to 0°C when an electric field strength of 15 MV / m is applied, and there is no sign reversal within this temperature range. For samples with m in the range of 0.8<m≤0.95, a negative electrothermal effect is exhibited under this temperature range and electric field strength, but there is no sign reversal.
[0184] In Figure 9 the temperature dependence of the adiabatic temperature change of Sample No. 2 and Sample No. 6 when an electric field of 15 MV / m is applied is presented. (In addition, as in Figure 7As shown, for sample number 1, the results of measuring the adiabatic temperature change with a larger electric field strength (20 MV / m) indicate that its thermoelectric effect is small in the temperature range below 0℃, therefore the comparison is omitted here.
[0185] like Figure 9 As shown, if it is sample number 6 within the scope of this invention, excellent adiabatic temperature variation can be obtained over a wide temperature range below room temperature, such as 0°C to -50°C. Therefore, it can be seen that the ceramic of this disclosure is suitable for applications requiring operation at low temperatures, such as refrigerators and freezers.
[0186] When the value of m is less than 0.6, the ferroelectric transition temperature does not decrease sufficiently. When m is greater than 0.95, the transition temperature does not decrease sufficiently. In addition, the threshold voltage of the antiferroelectric is not reduced. Therefore, it can be considered that the adiabatic temperature change under low temperature and low electric field is smaller.
[0187] Tables 2, 3 and 4 show the results of the thermoelectric effect of ceramics expressed by equation (1) for m = 0.6, m = 0.8 and m = 0.95, respectively.
[0188] Regarding samples where m falls within the scope of this invention, the most stable condition is when both x and y are near 0, and the proportion of material with the desired crystal structure is close to 100%. Even when neither x nor y is near 0, no heterogeneous phase is generated; however, if the deviation from 0 is significant, the proportion of heterogeneous phase increases, or the insulation decreases, and component breakdown occurs when an electric field is applied (see the crystal structure column in Tables 2 to 4). However, as long as the composition falls within the scope of this invention, the main component can achieve the desired structure, and the absolute values of the adiabatic temperature changes when electric fields of 8 MV / m and 15 MV / m are applied at -15°C are 0.8 K and 1.5 K or more, respectively.
[0189] exist Figure 10 The results of the characteristic tests in Table 2 show the range of x and y components that form the basis of the Go criteria. For example... Figure 10 As shown, it can be confirmed that ceramics within the scope of this invention are rated as Go in the characteristic tests. Furthermore, Tables 3 and 4 also show... Figure 10 The same result.
[0190] Industrial availability
[0191] The thermoelectric effect element disclosed herein can exhibit a high thermoelectric effect, and therefore can be used, for example, as a thermal management element in electric vehicles or hybrid vehicles, air conditioners (e.g., air conditioners for electric vehicles or hybrid vehicles, air conditioners used as heat pumps, etc.), refrigerators or freezers, etc. In addition, it can be used as a cooling device for various electronic devices (e.g., small electronic devices such as portable phones, smartphones, tablet terminals, hard disk drives or data servers, or personal computers (PCs) where thermal countermeasures are significant).
[0192] Explanation of reference numerals in the attached figures
[0193] 1: Thermoelectric effect element;
[0194] 2a, 2b: Electrode layers;
[0195] 4: Ceramic layer;
[0196] 6: Layered bodies;
[0197] 8a, 8b: External electrodes.
Claims
1. A ceramic represented by formula (1), (1-m)PbSc 0.5-x Ta 0.5+x O3-mPbMg 0.5-y W 0.5+y O3 (1) In formula (1), m satisfies 0.60≤m≤0.95, when 0≤x and 0≤y, x≤0.1, y≤0.1 and 0≤x+y≤0.13 are satisfied, when 0>x and 0≤y, -0.1≤x<0 and 0≤y≤0.1 are satisfied, when 0≥x and 0>y, -0.1≤x, -0.1≤y and -0.13≤x+y<0 are satisfied, when 0<x and 0>y, 0<x≤0.1 and -0.1≤y<0 are satisfied.
2. The ceramic according to claim 1, wherein In the formula, when 0≤x and 0≤y, 0≤x+y≤0.1 is satisfied, when 0≥x and 0>y, -0.1≤x+y<0 is satisfied.
3. The ceramic according to claim 1 or 2, wherein In the formula, x is 0, and y is 0.
4. The ceramic according to claim 1 or 2, wherein In the formula, m satisfies 0.6≤m≤0.
9.
5. The ceramic according to claim 1 or 2, wherein The crystal structure of the ceramic has a perovskite structure.
6. A thermoelectric effect element, in which noble metal electrodes and the ceramic according to any one of claims 1 to 5 are alternately stacked.
7. The thermoelectric effect element according to claim 6, wherein The noble metal electrode is formed of Pt.
8. An electronic component, configured to have the thermoelectric effect element according to claim 6 or 7.
9. An electronic device, configured to have the thermoelectric effect element according to claim 6 or 7, or the electronic component according to claim 8.
Citation Information
Patent Citations
Electrocaloric effect element
WO2021131142A1