BP (Back Propagation) membrane loaded with metal organic framework and preparation method of BP membrane

By using the combination of zinc nitrate and cobalt ions, graphene oxide and polymer matrix crosslinking agent in BP membrane, the metal organic framework and membrane structure are optimized, and the problem of low selectivity and permeability of BP membrane is solved and the stability of the membrane is improved It has a good performance and separation effect, suitable for large-scale factory use and environmental protection.

CN118874231AActive Publication Date: 2024-11-01WUHAN XINFUYI PHOTOELECTRIC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411111033.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing BP films containing metal organic frameworks have low selectivity and permeability to carbon dioxide gas, and the compatibility between the metal organic frameworks and matrix membranes is poor, which affects the stability and separation effect of the membrane.

Method used

Using zinc nitrate and cobalt ions as metal organic framework materials, combining specific graphene oxide and polymer matrix crosslinkers, optimize the membrane structure through sonication and layered structure, improve the selectivity and permeability of the membrane, and grow zinc through the growth of zinc The base metal organic framework is then coated with the cobalt-based metal organic framework to optimize the channel structure and energy barrier.

Benefits of technology

It significantly improves the selectivity and permeability of the BP film to carbon dioxide gas, enhances the stability and durability of the film, avoids the problem of membrane separation and bubbling, is suitable for large-scale factory use, effectively reduces environmental pollution, and has important carbon Neutralization and climate change response significance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993146610000131
    Figure BDA0004993146610000131
Patent Text Reader

Abstract

The invention provides a BP film loaded with a metal organic framework and a preparation method thereof. The BP film loaded with the metal organic framework is prepared from the following raw materials: a metal organic framework material and a matrix solution. The metal organic framework material is prepared from the following raw materials: nitrate, imidazole and graphene oxide. The matrix solution is prepared from the following raw materials: polyethylene glycol monomethyl ether acrylate, polyethylene glycol diacrylate and a cross-linking agent. The prepared BP membrane loaded with the metal organic framework has high permeability and selectivity to carbon dioxide gas, the process is simple, and the compatibility between the metal organic framework and the matrix membrane is improved, so that a monolithic membrane material can be prepared, the problem of bubbling during separation of a membrane layer is avoided, and the stability and durability of the BP membrane are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of separation membranes, and in particular relates to a BP membrane carrying a metal organic framework and a preparation method thereof. Background Art

[0002] With the acceleration of global industrialization and the continuous growth of energy demand, the continuous increase in carbon dioxide (CO2) emissions has become one of the main causes of global warming. Therefore, effective control and reduction of CO2 emissions, as well as efficient capture and separation of CO2 from industrial waste gas, are of great significance for mitigating the greenhouse effect and achieving sustainable development. In this context, membrane separation technology has become a research hotspot in the field of CO2 separation due to its energy-saving, high efficiency, clean and environmentally friendly characteristics. Bipolar membrane (BP membrane) is an ion exchange membrane with a special structure. It can simultaneously generate hydrogen ions (H+) and hydroxide ions (OH-) under the action of an electric field, thereby achieving the simultaneous generation of acid and base during electrodialysis. Metal organic frameworks (MOFs) are porous crystalline materials with a periodic network structure formed by self-assembly of metal ions or metal clusters and organic ligands through coordination bonds. MOFs have significant characteristics such as high specific surface area, high porosity, adjustable pore size, and strong structural designability. These characteristics make them show great application potential in gas separation, storage, catalysis and other fields. Especially in gas separation, MOFs have a highly selective adsorption effect on specific gas molecules (such as CO2) due to their unique pore structure and chemical properties, making them one of the ideal materials for achieving efficient gas separation. Although bipolar membranes in the traditional sense are mainly used in fields such as water electrolysis to produce hydrogen or acid-base recovery, the composite membrane formed by introducing MOFs into BP membranes can be used for CO2 separation.

[0003] However, in the prior art, the prepared composite membrane not only has low selectivity and permeability to carbon dioxide gas, which affects the separation effect, but also has poor compatibility between the metal organic framework and the matrix membrane material, which further affects the life and stability of the BP membrane. Summary of the invention

[0004] The purpose of the present invention is to provide a BP membrane loaded with a metal organic framework and a preparation method thereof. The BP membrane loaded with a metal organic framework has high permeability and selectivity to carbon dioxide gas, and the process is simple, thereby improving the compatibility between the metal organic framework and the matrix membrane, thereby improving the stability and durability of the BP membrane.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A BP membrane loaded with a metal organic framework, the preparation raw materials of which include metal organic framework material and matrix solution.

[0007] Preferably, the raw materials for preparing the metal organic framework material include nitrate, imidazole and graphene oxide.

[0008] Preferably, the raw materials for preparing the matrix solution include polyethylene glycol monomethyl ether acrylate, polyethylene glycol diacrylate, and a cross-linking agent.

[0009] Preferably, the metal organic framework material accounts for 2% to 10% of the mass of the BP membrane.

[0010] Preferably, the average thickness of the BP film is 130-170 μm.

[0011] Preferably, the nitrate comprises zinc nitrate and cobalt nitrate.

[0012] Preferably, the molar ratio of zinc nitrate to cobalt nitrate is 1:(0.5-2).

[0013] Preferably, the imidazole is 2-methylimidazole.

[0014] Preferably, the molar ratio of the nitrate to imidazole is 1:(6-12).

[0015] The inventor selected zinc nitrate as one of the raw materials, and the prepared zinc-based metal organic framework material was applied to the PB membrane, which can improve the selectivity and permeability of the BP membrane to carbon dioxide. This is because the zinc-based metal organic framework material has a high specific surface area, which can expand a larger free volume in the organic matrix prepared in this application, strengthen the gas permeability of the prepared BP membrane, and at the same time, the pore size of the zinc-based metal organic framework material is consistent with the kinetic diameter of the carbon dioxide molecule, thereby improving the gas selectivity. However, the selectivity of the zinc-based metal organic framework for carbon dioxide is limited, and the BP membrane prepared only by the zinc-based metal organic framework has a poor separation effect on carbon dioxide.

[0016] The inventors found that, on the basis of introducing zinc ions, introducing appropriate cobalt ions can improve the permeability of BP membrane to carbon dioxide gas while also improving its selectivity. This may be because there is a synergistic effect between the two ions. On the one hand, the different coordination modes and spatial arrangements of cobalt and zinc may form channels with specific sizes and shapes, which can selectively allow carbon dioxide molecules to pass through while repelling other gas molecules. On the other hand, certain oxidation states of cobalt may form active sites on the surface of the metal organic framework, which can interact with carbon dioxide molecules and enhance the adsorption capacity of the metal organic framework to carbon dioxide. At the same time, the coordination environment of zinc can regulate the number and distribution of these active sites, thereby further optimizing its adsorption performance. In addition, the introduction of cobalt and zinc together may lead to the formation of different energy barriers and diffusion channels inside the metal organic framework, thereby affecting the diffusion and adsorption rate of gas molecules in the metal organic framework, and then realizing the efficient separation of carbon dioxide. However, the compatibility between the framework material and the polymer matrix is ​​poor, which affects the stability of the BP membrane and the separation effect of carbon dioxide.

[0017] Preferably, the graphene oxide includes single-layer graphene oxide and multi-layer graphene oxide.

[0018] Preferably, the weight ratio of the single-layer graphene oxide to the multi-layer graphene oxide is (2-5):1; further preferably, it is 4:1.

[0019] Preferably, the average thickness of the single-layer graphene oxide is 0.5 to 1.2 nm, and the diameter is 4 to 7 μm.

[0020] Preferably, the multilayer graphene oxide has an average thickness of 1 to 3 nm, a diameter of 4 to 7 μm, and 2 to 5 layers.

[0021] In some preferred embodiments, the single-layer graphene oxide and the multi-layer graphene oxide are both purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd.

[0022] Preferably, the mass ratio of the graphene oxide to the nitrate is 1:(10-20).

[0023] In order to improve the separation effect and stability of the BP membrane, two specific graphene oxides were selected. This may be because, on the one hand, the specific single-layer graphene oxide and multi-layer graphene oxide were selected. They have similar diameters and little difference in thickness, so there is a certain compatibility between the two. On the one hand, the complementarity in the number of layers is achieved, which not only retains the high activity of the single-layer graphene oxide, but also improves the mechanical properties of the BP membrane. On the other hand, the single-layer and multi-layer graphene oxides of similar sizes are intertwined and stacked to form a stable three-dimensional network structure, which can improve the structural stability of the metal organic framework material, thereby further improving its separation effect. However, considering the agglomeration effect of graphene oxide, its addition amount should not be too much, and excessive graphene oxide may block the membrane pores and affect the separation effect.

[0024] Preferably, the average molecular weight of the polyethylene glycol monomethyl ether acrylate is 600-1400 Da; more preferably, it is 1000.

[0025] Preferably, the average molecular weight of the polyethylene glycol diacrylate is 300-800 Da; more preferably, it is 600.

[0026] In some preferred embodiments, the polyethylene glycol monomethyl ether acrylate and polyethylene glycol diacrylate are both purchased from Shanghai Yuanye Biotechnology Co., Ltd.

[0027] Preferably, the mass ratio of the polyethylene glycol monomethyl ether acrylate to the polyethylene glycol diacrylate is (1-3):1.

[0028] The inventors found that the selection of two specific polymer matrices for cross-linking can improve the selectivity and permeability of the BP membrane to carbon dioxide, and at the same time improve the mechanical properties of the BP membrane, making it more stable and durable. This may be because the ether oxygen bonds in these two specific substances can produce a strong dipole-quadrupole interaction with carbon dioxide molecules, thereby giving the BP membrane excellent affinity for carbon dioxide molecules, which helps the dissolution and diffusion of carbon dioxide molecules in the membrane and improves the permeation flux of carbon dioxide; and the polyethylene glycol segment is hydrophilic and can form hydrogen bonds with water-soluble gas carbon dioxide molecules to promote its permeation and diffusion in the membrane. In addition, the selection of a specific molecular weight makes the BP membrane obtained by the cross-linking reaction of the two organic substances have good flexibility and mechanical properties, which helps to reduce the stress concentration and rupture risk of the membrane during the separation process and improve the durability and stability of the membrane. By adjusting the parameters such as the ratio of the two organic substances, the type of cross-linking agent, and the temperature during cross-linking, when the metal organic framework material is introduced, the structure and performance of the membrane can be flexibly regulated, selectively allowing carbon dioxide molecules to pass through, while repelling other gas molecules, thereby improving the selectivity for carbon dioxide. This controllability helps to optimize the separation performance of the BP membrane for carbon dioxide.

[0029] Preferably, the cross-linking agent is one or more of azobisisobutyronitrile and benzoyl peroxide; more preferably, it is azobisisobutyronitrile.

[0030] Preferably, the added amount of the cross-linking agent is 0.5% to 1.5% of the total mass of polyethylene glycol monomethyl ether acrylate and polyethylene glycol diacrylate.

[0031] A method for preparing a BP membrane carrying a metal organic framework comprises the following steps:

[0032] S1. Preparation of metal organic framework material: Graphene oxide powder is mixed and ultrasonically dispersed in methanol aqueous solution, nitrate is added and ultrasonic treatment is continued for 4 to 7 hours, and then imidazole is added and ultrasonic treatment is carried out for 10 to 15 hours to obtain a suspension, and the solid is collected by centrifugation and dried;

[0033] S2. Preparation of matrix solution: Mix the raw materials and stir them ultrasonically for 4 to 6 hours to make the solution homogenous;

[0034] S3. Preparation of BP membrane: Add metal organic framework material to the matrix solution, ultrasonically stir for 4 to 6 hours to homogenize the solution, remove bubbles, fill the solution into two glass plates, control the thickness of the BP membrane by controlling the distance between the glass plates, let it stand at 65 to 75°C for 2 to 3 hours, take it out and cool it to room temperature, and separate the BP membrane from the glass plates.

[0035] The inventors found that the introduction of graphene oxide by a specific method can improve the permeability and selectivity of the BP membrane to carbon dioxide gas. This may be because the oxygen-containing functional groups rich in graphene oxide not only give it a high affinity for carbon dioxide gas molecules, enhancing the selectivity of the BP membrane to carbon dioxide gas, but also provide sites for the growth of metal organic frameworks, greatly increasing its dispersibility in organic matrix solutions, improving its compatibility with polymer matrix solutions, and thus improving the selectivity and permeability of the BP membrane. In addition, the unique layered structure of graphene oxide can promote the efficient penetration of gas molecules in the separation membrane matrix, achieve high flux, and further improve the gas permeation efficiency of the BP membrane.

[0036] In some preferred embodiments, the preparation of the metal organic framework material in step S1 can be further optimized as follows:

[0037] A1. Graphene oxide powder was mixed and ultrasonically dispersed in a methanol aqueous solution, zinc nitrate was added, and ultrasonic treatment was continued for 4 to 7 hours, and then imidazole was added and ultrasonic treatment was performed for 10 to 15 hours to obtain a suspension, and the solid was collected by centrifugation, washed with anhydrous methanol, and dried in a vacuum oven at 50 to 60° C. for 24 to 48 hours to obtain substance 1;

[0038] A2. Dissolve imidazole, substance one and cobalt nitrate in deionized water to obtain imidazole solution, substance one solution and cobalt nitrate solution respectively. Mix the substance one solution and the cobalt nitrate solution evenly and pour them into the imidazole solution. Stir for 10 to 20 minutes and then collect the solid by centrifugation. Wash with deionized water and dry in a vacuum oven at 50 to 60° C. for 24 to 48 hours to obtain a metal organic framework material.

[0039] The inventors found that when preparing metal organic framework materials, cobalt ions and zinc ions are grown on graphene oxide at the same time. Although the selectivity of carbon dioxide will be improved to a certain extent, its permeability is limited. This may be because cobalt and zinc are introduced at the same time, and the active sites are more widely distributed, making the diffusion path of gas molecules in the membrane more complicated, which affects the permeability of carbon dioxide to a certain extent. The inventors found through a large number of experiments that by first growing a zinc-based metal organic framework on graphene oxide and then coating a layer of cobalt-based metal organic framework on the surface of the zinc-based metal organic framework, it is possible to further improve its permeability while improving the selectivity of carbon dioxide. This may be because cobalt is covered on the surface of zinc as a coating layer, which can make the cobalt sites on the surface of the membrane more concentrated, while the internal zinc sites are relatively few. This structure not only helps to form a specific surface chemical environment, has a stronger affinity and selectivity for carbon dioxide molecules, but also optimizes the pore structure, reduces the diffusion resistance of carbon dioxide molecules in the membrane, thereby improving its permeability.

[0040] Preferably, the solid-to-liquid ratio of the graphene oxide and the methanol aqueous solution is 1 g: (60-100) mL.

[0041] Preferably, the molar ratio of zinc nitrate to imidazole in step A1 is 1:(2-6).

[0042] Preferably, the molar ratio of cobalt nitrate to imidazole in step A2 is 1:(10-15).

[0043] Preferably, the solid-to-liquid ratio of the substance 1, cobalt nitrate and deionized water is 1 g: (30-50) mL.

[0044] Preferably, in step A2, the solid-liquid ratio of imidazole to deionized water is 1 g: (60-100) mL.

[0045] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0046] 1. The present invention provides a BP membrane loaded with a metal organic framework, which has high permeability and selectivity to carbon dioxide gas and a simple process, thereby improving the compatibility between the metal organic framework and the matrix membrane, thereby improving the compatibility between the metal organic framework and the matrix membrane, thereby producing a monolithic bipolar membrane material, avoiding the separation bubbling problem of the membrane layer, improving the stability and durability of the BP membrane, and being suitable for large-scale factory use. At the same time, carbon dioxide can be captured and separated through membrane separation technology to reduce environmental pollution, which is of great significance for achieving the goal of carbon neutrality and responding to climate change.

[0047] 2. The present invention uses zinc nitrate as one of the raw materials, and the prepared zinc-based metal organic framework material is applied to the PB membrane, which can improve the selectivity and permeability of the BP membrane to carbon dioxide.

[0048] 3. The present invention introduces appropriate cobalt ions on the basis of introducing zinc ions, which can improve the permeability of BP membrane to carbon dioxide gas and also improve its selectivity.

[0049] 4. The present invention introduces graphene oxide through a specific method, which can improve the permeability and selectivity of the BP membrane to carbon dioxide gas. At the same time, in order to improve the separation effect and stability of the BP membrane, two specific graphene oxides are selected.

[0050] 5. The present invention selects two specific polymer matrices for cross-linking, which can improve the selectivity and permeability of the BP membrane to carbon dioxide, and at the same time can improve the mechanical properties of the BP membrane, making it more stable and durable.

[0051] 6. The present invention can further improve the permeability of carbon dioxide while improving the selectivity of carbon dioxide by first growing a zinc-based metal organic framework on graphene oxide and then coating the surface of the zinc-based metal organic framework with a layer of cobalt-based metal organic framework. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] The raw materials used in the present invention are all commercially available, specifically:

[0054] The average thickness of single-layer graphene oxide is 0.5-1.2 nm, and the diameter is 4-7 μm; the average thickness of multi-layer graphene oxide is 1-3 nm, the diameter is 4-7 μm, and the number of layers is 2-5; all are purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd.

[0055] The average molecular weight of polyethylene glycol monomethyl ether acrylate is 1000 Da; the average molecular weight of polyethylene glycol diacrylate is 600 Da; both were purchased from Shanghai Yuanye Biotechnology Co., Ltd.

[0056] Example 1

[0057] This embodiment provides a BP membrane loaded with a metal organic framework, and the raw materials for preparing the BP membrane are a metal organic framework material and a matrix solution.

[0058] The raw materials for preparing the metal organic framework material are nitrate, imidazole, graphene oxide, methanol aqueous solution and deionized water.

[0059] The raw materials for preparing the matrix solution are polyethylene glycol monomethyl ether acrylate, polyethylene glycol diacrylate and a crosslinking agent.

[0060] The metal organic framework material accounts for 5% of the mass of the BP membrane.

[0061] The average thickness of the BP film was 150 μm.

[0062] The nitrates are zinc nitrate and cobalt nitrate.

[0063] The molar ratio of the zinc nitrate to the cobalt nitrate is 1:1.

[0064] The imidazole is 2-methylimidazole.

[0065] The molar ratio of the nitrate to imidazole is 1:8.

[0066] The graphene oxide is single-layer graphene oxide and multi-layer graphene oxide.

[0067] The weight ratio of the single-layer graphene oxide to the multi-layer graphene oxide is 4:1.

[0068] The mass ratio of the graphene oxide to the nitrate is 1:15.

[0069] The mass ratio of the polyethylene glycol monomethyl ether acrylate to the polyethylene glycol diacrylate is 2:1.

[0070] The cross-linking agent is azobisisobutyronitrile.

[0071] The added amount of the cross-linking agent is 1% of the total mass of polyethylene glycol monomethyl ether acrylate and polyethylene glycol diacrylate.

[0072] The preparation method of the BP membrane comprises the following steps:

[0073] S1. Preparation of metal organic framework materials;

[0074] S2. Preparation of matrix solution: Mix the raw materials and stir them ultrasonically for 5 hours to make the solution homogenous;

[0075] S3. Preparation of BP membrane: Add metal organic framework material to the matrix solution, stir ultrasonically for 5 hours to homogenize the solution, remove bubbles, fill the solution into two glass plates, control the thickness of the BP membrane by controlling the distance between the glass plates, let it stand at 70°C for 2.5 hours, take it out and cool it to room temperature, and separate the BP membrane from the glass plates.

[0076] The step S1 of preparing the metal organic framework material comprises the following steps:

[0077] A1. Graphene oxide powder was mixed and ultrasonically dispersed in a methanol aqueous solution, zinc nitrate was added, and ultrasonic treatment was continued for 5 h, and then imidazole was added and ultrasonic treatment was performed for 12 h to obtain a suspension, and the solid was collected by centrifugation, washed with anhydrous methanol, and dried in a vacuum oven at 55° C. for 36 h to obtain substance 1;

[0078] A2. Dissolve imidazole, substance 1 and cobalt nitrate in deionized water to obtain imidazole solution, substance 1 solution and cobalt nitrate solution respectively. Mix the substance 1 solution and the cobalt nitrate solution evenly and pour them into the imidazole solution. Stir for 15 minutes and then collect the solid by centrifugation. Wash with deionized water and dry in a vacuum oven at 55° C. for 36 hours to obtain a metal organic framework material.

[0079] The volume fraction of the methanol aqueous solution is 30%.

[0080] The solid-to-liquid ratio of the graphene oxide and the methanol aqueous solution is 1 g:80 mL.

[0081] The molar ratio of zinc nitrate to imidazole in step A1 is 1:4.

[0082] The molar ratio of cobalt nitrate to imidazole in step A2 is 1:12.

[0083] The solid-to-liquid ratio of the substance 1, cobalt nitrate and deionized water is 1 g:40 mL.

[0084] The solid-to-liquid ratio of imidazole to deionized water in step A2 is 1 g:80 mL.

[0085] Example 2

[0086] The difference between this embodiment and embodiment 1 is that the weight ratio of the single-layer graphene oxide to the multi-layer graphene oxide is 2:1.

[0087] Example 3

[0088] The difference between this embodiment and embodiment 1 is that the molar ratio of the nitrate to imidazole is 1:6; the molar ratio of zinc nitrate to imidazole in step A1 is 1:3; and the molar ratio of cobalt nitrate to imidazole in step A2 is 1:9.

[0089] Comparative Example 1

[0090] The difference between this comparative example and Example 1 is that the nitrate is zinc nitrate; S1. Preparation of metal organic framework material: graphene oxide powder is mixed and ultrasonically dispersed in a methanol aqueous solution, nitrate is added and ultrasonic treatment is continued for 5 hours, then imidazole is added and ultrasonic treatment is carried out for 12 hours to obtain a suspension, the solid is collected by centrifugation, washed with anhydrous methanol, and dried in a vacuum oven at 55°C for 36 hours to obtain.

[0091] Comparative Example 2

[0092] The difference between this comparative example and Example 1 is that the molar ratio of zinc nitrate to cobalt nitrate is 1:4; the molar ratio of nitrate to imidazole is 1:8; the molar ratio of zinc nitrate to imidazole in step A1 is 1:4; and the molar ratio of cobalt nitrate to imidazole in step A2 is 1:9.

[0093] Comparative Example 3

[0094] The difference between this comparative example and Example 1 is that the weight ratio of the single-layer graphene oxide to the multi-layer graphene oxide is 1:1.

[0095] Comparative Example 4

[0096] The difference between this comparative example and Example 1 is that the mass ratio of the graphene oxide to the nitrate is 1:5.

[0097] Comparative Example 5 - Uncoated

[0098] The difference between this comparative example and Example 1 is that the step S1 of preparing the metal organic framework material comprises the following steps: mixing graphene oxide powder and ultrasonically dispersing it in a methanol aqueous solution, adding nitrate, continuing ultrasonic treatment for 5 hours, then adding imidazole and ultrasonically treating for 12 hours to obtain a suspension, collecting the solid by centrifugation, washing it with anhydrous methanol, and drying it in a vacuum oven at 55°C for 36 hours to obtain the metal organic framework material.

[0099] Comparative Example 6 - Not grown on graphene oxide

[0100] The difference between this comparative example and Example 1 is that the preparation of the metal organic framework material in step S1 comprises the following steps:

[0101] A1. Dissolve imidazole and zinc nitrate in deionized water to obtain imidazole solution and zinc nitrate solution respectively. Mix and stir the two solutions for 5 hours, collect the solid by centrifugation, and dry in a vacuum oven at 55° C. for 12 hours to obtain substance 1.

[0102] A2, dissolving imidazole, substance 1 and cobalt nitrate in deionized water to obtain imidazole solution, substance 1 solution and cobalt nitrate solution respectively, mixing substance 1 solution and cobalt nitrate solution evenly and pouring into imidazole solution, stirring for 15 min and collecting solid by centrifugation, washing with deionized water and drying in a vacuum oven at 55° C. for 36 h to obtain substance 2;

[0103] A3. Graphene oxide powders were mixed and ultrasonically dispersed in a methanol aqueous solution, substance 2 was added, and ultrasonic treatment was performed for 15 h to obtain a suspension, solids were collected by centrifugation, washed with anhydrous methanol, and dried in a vacuum oven at 55° C. for 36 h.

[0104] The volume fraction of the methanol aqueous solution is 30%.

[0105] The solid-to-liquid ratio of the graphene oxide and the methanol aqueous solution is 1 g:80 mL.

[0106] The molar ratio of zinc nitrate to imidazole in step A1 is 1:4.

[0107] In the step A1, the solid-to-liquid ratio of zinc nitrate, imidazole and deionized water is 1 g:40 mL.

[0108] In step A2, the solid-liquid ratio of imidazole to deionized water is 1 g:80 mL, and the solid-liquid ratio of substance 1, cobalt nitrate and deionized water is 1 g:40 mL.

[0109] The molar ratio of cobalt nitrate to imidazole in step A2 is 1:12.

[0110] Comparative Example 7

[0111] The difference between this comparative example and Example 1 is that the average molecular weight of the polyethylene glycol diacrylate is 2000, which is purchased from Hubei Shineng Chemical Technology Co., Ltd.

[0112] Comparative Example 8: No graphene oxide added

[0113] The difference between this comparative example and Example 1 is that the preparation of the metal organic framework material in step S1 comprises the following steps:

[0114] A1. Dissolve imidazole and zinc nitrate in deionized water to obtain imidazole solution and zinc nitrate solution respectively. Mix and stir the two solutions for 5 hours, collect the solid by centrifugation, and dry in a vacuum oven at 55° C. for 12 hours to obtain substance 1.

[0115] A2. Dissolve imidazole, substance 1 and cobalt nitrate in deionized water to obtain imidazole solution, substance 1 solution and cobalt nitrate solution respectively. Mix the substance 1 solution and the cobalt nitrate solution evenly and pour them into the imidazole solution. Stir for 15 minutes and then collect the solid by centrifugation. Wash with deionized water and dry in a vacuum oven at 55°C for 36 hours to obtain the product.

[0116] Performance Testing

[0117] The selectivity and permeability of BP membrane for carbon dioxide gas were tested by referring to the method in the article "Study on the performance of two-dimensional vermiculite nanosheet mixed matrix membrane for separation of CO2 / CH4" published by Hou Jinpeng et al. At the same time, in order to measure the working stability of BP membrane, its selectivity for carbon dioxide gas was tested after working for 120 hours, and its change rate was calculated. The results are shown in Table 1.

[0118] Table 1 Measurement results

[0119]

[0120] According to statistics, the BP membranes loaded with metal organic frameworks prepared in Examples 1 to 3 of the present invention have high selectivity and permeability for carbon dioxide molecules, and still have high selectivity after working for 120 hours. Comparative Example 1 does not add cobalt nitrate, Comparative Example 2 has too high an addition of cobalt nitrate, Comparative Example 3 has relatively small additions of monolayer graphene oxide, Comparative Example 4 has too high an addition of graphene oxide, Comparative Example 5 does not undergo coating treatment, Comparative Example 6 MOF does not grow on graphene oxide, Comparative Example 7 has too high an average molecular weight of polyethylene glycol diacrylate, Comparative Example 8 does not add graphene oxide, and the prepared BP membrane has poor selectivity, permeability and stability for carbon dioxide gas. Therefore, the BP membrane loaded with metal organic frameworks prepared by the raw materials and methods described in this application has high permeability and selectivity for carbon dioxide gas, and the process is simple, the compatibility between the metal organic framework and the matrix membrane is good, and a monolithic membrane material can be prepared, avoiding the separation bubbling problem of the membrane layer, and improving the stability and durability of the BP membrane.

[0121] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A BP membrane loaded with a metal organic framework, characterized in that: The raw materials for preparing the metal organic framework-loaded BP membrane include metal organic framework materials and matrix solution; The raw materials for preparing the metal organic framework material include nitrate, imidazole and graphene oxide; The raw materials for preparing the matrix solution include polyethylene glycol monomethyl ether acrylate, polyethylene glycol diacrylate, and a cross-linking agent; The nitrates include zinc nitrate and cobalt nitrate; The molar ratio of zinc nitrate to cobalt nitrate is 1:(0.5-2); The imidazole is 2-methylimidazole; The molar ratio of the nitrate to imidazole is 1:(6-12); The graphene oxide includes single-layer graphene oxide and multi-layer graphene oxide; The weight ratio of the single-layer graphene oxide to the multi-layer graphene oxide is (2-5):1; The average thickness of the single-layer graphene oxide is 0.5 to 1.2 nm, and the diameter is 4 to 7 μm; The multilayer graphene oxide has an average thickness of 1 to 3 nm, a diameter of 4 to 7 μm, and 2 to 5 layers; The mass ratio of the graphene oxide to the nitrate is 1:(10-20).

2. The BP membrane loaded with a metal organic framework according to claim 1, characterized in that: The metal organic framework material accounts for 2% to 10% of the mass of the BP membrane.

3. The BP membrane carrying a metal organic framework according to claim 1, characterized in that: The average thickness of the BP film is 130-170 μm.

4. The BP membrane carrying a metal organic framework according to claim 1, characterized in that: The average molecular weight of the polyethylene glycol monomethyl ether acrylate is 600-1400 Da.

5. The BP membrane carrying a metal organic framework according to claim 4, characterized in that: The average molecular weight of the polyethylene glycol diacrylate is 300-800 Da.

6. The BP membrane carrying a metal organic framework according to claim 5, characterized in that: The mass ratio of the polyethylene glycol monomethyl ether acrylate to the polyethylene glycol diacrylate is (1-3):

1.

7. A method for preparing a BP membrane carrying a metal organic framework according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Preparation of metal organic framework material: Graphene oxide powder is mixed and ultrasonically dispersed in methanol aqueous solution, nitrate is added and ultrasonic treatment is continued for 4 to 7 hours, and then imidazole is added and ultrasonic treatment is carried out for 10 to 15 hours to obtain a suspension, and the solid is collected by centrifugation and dried; S2. Preparation of matrix solution: Mix the raw materials and stir them ultrasonically for 4 to 6 hours to make the solution homogenous; S3. Preparation of BP membrane: Add metal organic framework material to the matrix solution, ultrasonically stir for 4 to 6 hours to homogenize the solution, remove bubbles, fill the solution into two glass plates, control the thickness of the BP membrane by controlling the distance between the glass plates, let it stand at 65 to 75°C for 2 to 3 hours, take it out and cool it to room temperature, and separate the BP membrane from the glass plates.

8. The method for preparing a BP membrane carrying a metal organic framework according to claim 7, characterized in that: The preparation method of step S1 comprises the following steps: A1. Graphene oxide powder was mixed and ultrasonically dispersed in a methanol aqueous solution, zinc nitrate was added, and ultrasonic treatment was continued for 4 to 7 hours, and then imidazole was added and ultrasonic treatment was performed for 10 to 15 hours to obtain a suspension, and the solid was collected by centrifugation, washed with anhydrous methanol, and dried in a vacuum oven at 50 to 60° C. for 24 to 48 hours to obtain substance 1; A2. Dissolve imidazole, substance one and cobalt nitrate in deionized water to obtain imidazole solution, substance one solution and cobalt nitrate solution respectively. Mix the substance one solution and the cobalt nitrate solution evenly and pour them into the imidazole solution. Stir for 10 to 20 minutes and then collect the solid by centrifugation. Wash with deionized water and dry in a vacuum oven at 50 to 60° C. for 24 to 48 hours to obtain a metal organic framework material.

9. The method for preparing a BP membrane carrying a metal organic framework according to claim 8, characterized in that: The molar ratio of zinc nitrate to imidazole in step A1 is 1:(2-6).

10. The method for preparing a BP membrane carrying a metal organic framework according to claim 8, characterized in that: The molar ratio of cobalt nitrate to imidazole in step A2 is 1:(10-15).

Citation Information

Patent Citations

  • Polyimide-zinc organic framework loaded graphene oxide hybrid membrane as well as preparation and application

    CN107866154A

  • Graphene oxide / metal organic frame composite film, preparation method and application thereof

    CN110270234A

  • Metal-organic framework-loaded graphene microsphere as well as preparation method and application thereof

    CN111704732A

  • Stretchable electrochemical harvester and manufacturing method thereof

    KR102797942B1