Narrow gap welding process method for hydraulic support stand column middle cylinder

By adopting narrow gap welding process and pulse power supply technology in hydraulic support columns, the problem of welding defects during the welding process of S890Q steel plates is solved, the weld strength and stability are improved, the product design requirements are met, and the welding materials and production are saved cost.

CN118875431APending Publication Date: 2024-11-01PINGDINGSHAN COAL MINE MACHINERY EQUIP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411103642.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When using S890Q high-strength steel plates in hydraulic support columns, welding defects are prone to occur during welding, resulting in insufficient strength of the weld and unable to meet the design requirements.

Method used

The narrow gap welding process method includes turning U-shaped bevels at the bottom and middle cylinder, using pulse power supply and specific welding wires (ER69-G and ER76-G), preheating and protecting gases to reduce crack sensitivity, And the welding heat input is controlled through multi-layer multi-pass welding to ensure the strength and stability of the weld.

Benefits of technology

It effectively solves the problem of welding defects, improves the tensile strength of the weld, meets product usage requirements, saves welding materials and production costs, and ensures product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875431A_ABST
    Figure CN118875431A_ABST
Patent Text Reader

Abstract

The invention relates to a narrow gap welding process method for a hydraulic support stand column middle cylinder. The narrow gap welding process method comprises the processes of groove making, to-be-welded area cleaning, pulse welding power source using, welding wire selecting according to the low-strength matching principle, welding through a circular seam welding cylinder machine and the like. The method is reasonable and feasible, a narrow gap groove is selected, a large amount of weld metal is saved, the welding workload is reduced, a pulse power supply is used, the problem of poor root fusion is solved, and in general, the problem of weldability of an existing hydraulic support stand column S890Q middle cylinder is solved. Compared with the prior art, the device has good market prospect and development space.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydraulic support column jack welding, and in particular to a narrow gap welding process method for a hydraulic support column cylinder and a metering method thereof. Background Art

[0002] In recent years, with the advancement of technology and the rapid development of the coal mining industry, the mining height of hydraulic supports has become larger and larger, the working resistance has also been continuously increased, and the service life requirements of columns have been greatly improved. Some new materials (such as S890Q high-strength steel plates) have also begun to be used in large-diameter columns. Due to structural limitations, this type of steel needs to be welded during use. This type of steel has a complex alloy system, contains many trace elements, and the carbon equivalent CE is generally above 0.6%. It has a strong tendency to harden and has an obvious tendency to cold cracks. It is easy to have root cracks, and it is also easy to have embrittlement and softening of the heat-affected zone. How to obtain a welded joint with stable quality is the key to the successful application of this type of steel. The design technology of hydraulic support columns requires that the tensile strength of the S890Q material weld is not less than 800MPa. This type of steel is prone to welding defects during welding, resulting in insufficient weld strength and unable to meet the design requirements. It is crucial to study the weldability of this type of steel and formulate a suitable welding process. Summary of the invention

[0003] In order to solve the technical problems that welding defects are prone to occur in the welding process of the existing S890Q material for columns, resulting in insufficient weld strength and failure to meet design requirements, the present invention provides a narrow gap welding process method for the cylinder of a hydraulic support column. The method is reasonable and feasible, and a narrow gap groove is selected to save a large amount of weld metal and reduce welding workload. A pulse power supply is used to solve the problem of poor root fusion, meet product use requirements, and ensure product quality.

[0004] The technical solution adopted by the present invention to solve the above technical problems is: a narrow gap welding process method for a hydraulic support column cylinder, comprising the following steps: Step 1: First, make a U-shaped groove on the test piece. According to the drawing, turn the U-shaped groove at the connection between the middle cylinder bottom and the middle cylinder barrel; Step 2: Secondly, surface grinding: Use a hand-held grinder to grind and clean the inside and sides of the groove of the test piece within a range of about 20 mm to present a metallic luster; Step 3: Preheat before welding. Use a baking gun to heat the position to be welded for 2-5 minutes, heat it to 100-150℃, and measure the temperature with an infrared spot thermometer. Step 4, then, welding is carried out. The specimen is welded by a girth welding cylinder machine. A pulse power supply is used for the welding power supply. A shielding gas is filled in with a gas flow rate of 20-25L / min. Multi-layer and multi-pass welding is adopted to control the welding heat input. The interlayer temperature of the weld is ≤250℃. ER69-G welding wire is used for the base welding to reduce the crack sensitivity. ER76-G welding wire is used for the filling and capping welding to ensure the strength of the weld. Step 5: After welding, wrap the welded steel sheet with a blanket to keep it warm for 1-2 hours, and then cool it in the air. After cooling, perform appearance inspection and ultrasonic flaw detection. Step six, conduct mechanical property tests on qualified specimens, including tensile property tests, bending property tests and impact property tests.

[0005] As a further optimization scheme of the above-mentioned narrow gap welding process method for the middle cylinder of the hydraulic support column, the U-shaped groove turned in the step one respectively turns a section of relatively positioned J-shaped grooves at the middle cylinder bottom and the connecting part of the middle cylinder barrel specimen, and the two groups of J-shaped grooves relatively form an annular U-shaped groove.

[0006] As a further optimization scheme of the above-mentioned narrow gap welding process method for the cylinder of the hydraulic support column, the bottom of the U-shaped groove is a semicircular arc structure, the bottom radius of the U-shaped groove is 5mm, the depth of the U-shaped groove is 30-60mm, and the width of the U-shaped groove is 11-13mm.

[0007] As a further optimization scheme of the above-mentioned narrow gap welding process method for the cylinder of the hydraulic support column, the shielding gas in step 4 is a mixed gas of 80% Ar+20% CO2.

[0008] As a further optimization scheme of the above-mentioned narrow gap welding process method for the cylinder of the hydraulic support column, the appearance inspection in step five does not show any cracks, pores, undercuts, or arc pits in the welding defects; and the ultrasonic flaw detection does not show any out-of-range defects.

[0009] As a further optimization scheme of the above-mentioned narrow gap welding process method for the cylinder of the hydraulic support column, the material of the test piece is selected from S890Q high-strength steel plate.

[0010] Compared with the prior art, the present invention has the following beneficial effects: First, in the process of the present invention, the low-strength matching principle is adopted (ER69-G welding wire is used for base welding, and ER76-G welding wire is used for filling and capping welding). ER69-G welding wire is used for base welding, and the welding wire has low strength, and cold cracks are not easy to occur at the root, thereby avoiding welding defects; ER76-G welding wire is used for filling and capping welding to ensure the strength of the weld, so that it meets the product use requirements, thus taking both into account.

[0011] Second, in the process of the present invention, the welding groove is in the form of a narrow gap U-shaped groove. This groove form saves welding materials, and correspondingly reduces welding gas consumption and power consumption, saving production costs.

[0012] Third, in the process of the present invention, a pulse welding machine is used, and the stirring and digging effect of the pulse on the molten pool is utilized to ensure good fusion of the root of the weld, solve the problem of poor root fusion, and stabilize product quality.

[0013] Fourth, the present invention solves the technical problem that the S890Q middle cylinder of the column is difficult to weld, and lays a foundation for the successful use of this material. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic diagram of the position of the weld to be welded in the column center cylinder; Figure 2 This is a schematic diagram of the welding specimen joint form; Figure 3 Schematic diagram of the welding sequence of the welded specimen joint. DETAILED DESCRIPTION

[0015] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0016] Embodiment 1, a narrow gap welding process method for a hydraulic support column cylinder, comprising the following steps: Step 1: First, make a U-shaped groove on the test piece. According to the drawing, turn the U-shaped groove at the connection between the middle cylinder bottom and the middle cylinder barrel; Step 2: Secondly, surface grinding: Use a hand-held grinder to grind and clean the inside and sides of the groove of the test piece within a range of about 20 mm to present a metallic luster; Step 3: Preheat before welding. Use a baking gun to heat the position to be welded for 2 minutes, heat it to 100°C, and measure the temperature with an infrared spot thermometer. Step 4: Then, welding is performed. The specimen is welded using a girth welding cylinder machine. A pulse power supply is used as the welding power source. Shielding gas is filled in with a gas flow rate of 20 L / min. Six layers and six passes are used to control the welding heat input. The weld interlayer temperature is ≤250°C. ER69-G welding wire is used for base welding to reduce crack sensitivity. ER76-G welding wire is used for filling and capping welding to ensure the strength of the weld. Step 5: After welding, wrap the welded steel sheet with a quilt to keep it warm for 1 hour, and then cool it in the air. After cooling, it will be inspected by appearance and ultrasonic testing. Step six, conduct mechanical property tests on qualified specimens, including tensile property tests, bending property tests and impact property tests.

[0017] The U-shaped groove machined in step 1 is respectively machined into a relatively positioned J-shaped groove at the middle cylinder bottom and the connecting portion of the middle cylinder barrel specimen, and two groups of J-shaped grooves relatively form an annular U-shaped groove.

[0018] The bottom of the U-shaped groove is a semicircular arc structure, the bottom radius of the U-shaped groove is 5 mm, the depth of the U-shaped groove is 30 mm, and the width of the U-shaped groove is 11 mm.

[0019] The protective gas in step 4 is a mixed gas of 80% Ar + 20% CO2.

[0020] The appearance inspection in step 5 does not reveal any cracks, pores, undercuts, or arc pits in welding defects; and the ultrasonic flaw detection does not reveal any defects beyond the range.

[0021] The material of the test piece is S890Q high-strength steel plate.

[0022] Embodiment 2, a narrow gap welding process method for a hydraulic support column cylinder, comprising the following steps: Step 1: First, make a U-shaped groove on the test piece. According to the drawing, turn the U-shaped groove at the connection between the middle cylinder bottom and the middle cylinder barrel; Step 2: Secondly, surface grinding: Use a hand-held grinder to grind and clean the inside and sides of the groove of the test piece within a range of about 20 mm to present a metallic luster; Step 3: Preheat before welding. Use a baking gun to heat the welding position for 3 minutes, heat it to 120°C, and measure the temperature with an infrared spot thermometer. Step 4: Then, welding is performed. The specimen is welded using a girth welding cylinder machine. A pulse power supply is used as the welding power source. Shielding gas is filled in with a gas flow rate of 23L / min. Six layers and six passes are used to control the welding heat input. The weld interlayer temperature is ≤250°C. ER69-G welding wire is used for base welding to reduce crack sensitivity. ER76-G welding wire is used for filling and capping welding to ensure the strength of the weld. Step 5: After welding, wrap the welded steel sheet with a quilt to keep it warm for 1.5 hours and then cool it in the air. After cooling, it will be inspected by appearance and ultrasonic testing. Step six, conduct mechanical property tests on qualified specimens, including tensile property tests, bending property tests and impact property tests.

[0023] The U-shaped groove machined in step 1 is respectively machined into a relatively positioned J-shaped groove at the middle cylinder bottom and the connecting portion of the middle cylinder barrel specimen, and two groups of J-shaped grooves relatively form an annular U-shaped groove.

[0024] The bottom of the U-shaped groove is a semicircular arc structure, the bottom radius of the U-shaped groove is 5 mm, the depth of the U-shaped groove is 45 mm, and the width of the U-shaped groove is 12 mm.

[0025] The protective gas in step 4 is a mixed gas of 80% Ar + 20% CO2.

[0026] The appearance inspection in step 5 does not reveal any cracks, pores, undercuts, or arc pits in welding defects; and the ultrasonic flaw detection does not reveal any defects beyond the range.

[0027] The material of the test piece is S890Q high-strength steel plate.

[0028] Embodiment 3, a narrow gap welding process method for a hydraulic support column cylinder, comprising the following steps: Step 1: First, make a U-shaped groove on the test piece. According to the drawing, turn the U-shaped groove at the connection between the middle cylinder bottom and the middle cylinder barrel; Step 2: Secondly, surface grinding: Use a hand-held grinder to grind and clean the inside and sides of the groove of the test piece within a range of about 20 mm to present a metallic luster; Step 3: Preheat before welding. Use a baking gun to heat the position to be welded for 5 minutes, heat it to 150°C, and measure the temperature with an infrared spot thermometer. Step 4: Then, welding is performed. The specimen is welded using a girth welding cylinder machine. A pulse power supply is used as the welding power source. Shielding gas is filled in with a gas flow rate of 25 L / min. Six layers and six passes are used to control the welding heat input. The weld interlayer temperature is ≤250°C. ER69-G welding wire is used for base welding to reduce crack sensitivity. ER76-G welding wire is used for filling and capping welding to ensure the strength of the weld. Step 5: After welding, wrap the welded steel sheet with a quilt to keep it warm for 2 hours, and then cool it in the air. After cooling, it will be inspected by appearance and ultrasonic testing. Step six, conduct mechanical property tests on qualified specimens, including tensile property tests, bending property tests and impact property tests.

[0029] The U-shaped groove machined in step 1 is respectively machined into a relatively positioned J-shaped groove at the middle cylinder bottom and the connecting portion of the middle cylinder barrel specimen, and two groups of J-shaped grooves relatively form an annular U-shaped groove.

[0030] The bottom of the U-shaped groove is a semicircular arc structure, the bottom radius of the U-shaped groove is 5 mm, the depth of the U-shaped groove is 60 mm, and the width of the U-shaped groove is 13 mm.

[0031] The protective gas in step 4 is a mixed gas of 80% Ar + 20% CO2.

[0032] The appearance inspection in step 5 does not reveal any cracks, pores, undercuts, or arc pits in welding defects; and the ultrasonic flaw detection does not reveal any defects beyond the range.

[0033] The material of the test piece is S890Q high-strength steel plate.

[0034] In actual operation, in step 4, the test piece is welded with a girth welding cylinder machine, a pulse power supply is used for the welding power supply, and multi-layer and multi-pass welding is adopted to control the welding heat input. The thermal cycle between weld layers can eliminate some stress and structural defects. The interlayer temperature is ≤250℃. ER69-G welding wire is used for base welding to reduce crack sensitivity as much as possible, and ER76-G welding wire is used for filling and capping welding to ensure the strength of the weld.

[0035] See attached for welding sequence Figure 3 , at least 4 passes are required for welding, and as the circumference diameter increases, the number of welding layers also increases. The welding parameters are shown in Table 1.

[0036] Table 1 shows the specific welding parameters of the welding specimens. In step 5, the appearance inspection after welding is qualified, and the visual inspection meets the requirements of ISO5817-B. There shall be no welding defects such as cracks, pores, undercuts, arc pits, etc. Ultrasonic flaw detection is carried out after 48 hours. The ultrasonic flaw detection results meet ISO11666-2 level and there are no defects beyond the scope; The specimens welded according to the above process were subjected to tensile, bending and impact tests according to ISO15614-1 standard. The results are shown in Table 2.

[0037] Table 2 is the test results of mechanical properties of S890Q steel butt joints It can be seen that the tensile strength of the weld exceeds 800MPa, the bending is qualified, and the impact toughness is excellent. This welding process is applied to the welding production of the S890Q cylinder of the hydraulic support column, which meets the product technical requirements and solves the weldability problem of the S890Q cylinder of the column.

[0038] The method of the present invention is reasonable and feasible, selects narrow gap grooves, saves a lot of weld metal, reduces welding workload, uses pulse power supply, meets product use requirements, ensures product quality, and solves the technical problems of welding defects that are easy to occur in the welding process of existing column S890Q materials, resulting in insufficient weld strength and failure to meet design requirements. It has very important positive significance and market prospects for the existing technology.

[0039] The preferred specific implementation modes and embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes and embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present invention.

Claims

1. A narrow gap welding process for a hydraulic support column cylinder, characterized in that: The following steps are included: Step 1: First, make a U-shaped groove on the test piece. According to the drawing, turn the U-shaped groove at the connection between the middle cylinder bottom and the middle cylinder barrel; Step 2: Secondly, surface grinding: Use a hand-held grinder to grind and clean the inside and sides of the groove of the test piece within a range of about 20 mm to present a metallic luster; Step 3: Preheat before welding. Use a baking gun to heat the position to be welded for 2-5 minutes, heat it to 100-150℃, and measure the temperature with an infrared spot thermometer. Step 4, then, welding is carried out. The specimen is welded by a girth welding cylinder machine. A pulse power supply is used for the welding power supply. A shielding gas is filled in with a gas flow rate of 20-25L / min. Multi-layer and multi-pass welding is adopted to control the welding heat input. The interlayer temperature of the weld is ≤250℃. ER69-G welding wire is used for the base welding to reduce the crack sensitivity. ER76-G welding wire is used for the filling and capping welding to ensure the strength of the weld. Step 5: After welding, wrap the welded steel sheet with a quilt to keep it warm for 1-2 hours, and then cool it in the air. After cooling, it will be inspected by appearance and ultrasonic testing. Step six, conduct mechanical property tests on qualified specimens, including tensile property tests, bending property tests and impact property tests.

2. A narrow gap welding process for a hydraulic support column cylinder as claimed in claim 1, characterized in that: The U-shaped groove machined in step 1 is respectively machined into a relatively positioned J-shaped groove at the middle cylinder bottom and the connecting portion of the middle cylinder barrel specimen, and two groups of J-shaped grooves relatively form an annular U-shaped groove.

3. A narrow gap welding process for a hydraulic support column cylinder as claimed in claim 2, characterized in that: The bottom of the U-shaped groove is a semicircular arc structure, the bottom radius of the U-shaped groove is 5mm, the depth of the U-shaped groove is 30-60mm, and the width of the U-shaped groove is 11-13mm.

4. A narrow gap welding process for a hydraulic support column cylinder as claimed in claim 1, characterized in that: The protective gas in step 4 is a mixed gas of 80% Ar + 20% CO2.

5. A narrow gap welding process for a hydraulic support column cylinder as claimed in claim 1, characterized in that: The appearance inspection in step 5 does not reveal any cracks, pores, undercuts, or arc pits in welding defects; and the ultrasonic flaw detection does not reveal any defects beyond the range.

6. A narrow gap welding process for a hydraulic support column cylinder according to any one of claims 1 to 5, characterized in that: The material of the specimen is S890Q high-strength steel plate.

Citation Information

Patent Citations

  • Narrow gap groove of steel containment vessel of nuclear power station and automatic welding method thereof

    CN103394796A

  • Coal mine hydraulic support oil cylinder narrow gap welding seam defect restraining method

    CN115533259A

  • Bridge steel thick plate narrow gap butt joint form and welding method

    CN116117283A

  • Welding method of crane boom body

    CN117259910A

  • Method for welding hollow main shaft and solid shaft head

    WO2016173314A1