Nickel-copper alloy coiled plate annealing and pickling line continuous production method

By using argon-oxygen mixture to protect the weld in the production of stainless steel continuous annealing and pickling line of nickel-copper alloy, selecting appropriate connecting materials and welding wires, and controlling welding parameters, the problems of Monel 400 alloy are solved. Continuous and stable production of nickel-copper alloy roll plates has been achieved.

CN118875438APending Publication Date: 2024-11-01GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213709.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Monel 400 alloy is difficult to weld in the production of stainless steel continuous annealing pickling line, and is prone to vicious accidents such as weld cracks and production line breakage, mainly due to the enrichment of Cu elements, resulting in liquefied cracks and pore defects.

Method used

Use argon-oxygen mixture to protect the weld, select appropriate connecting materials and fill wires, and control reasonable welding parameters, such as weld gap, voltage, wire feeding speed and torch height, automatically weld through MAG welding machine, and in the weld Cut the crescent at the arc starting and closing arc to ensure the quality of the welded joints.

Benefits of technology

It effectively avoids liquefied cracks in the welded joints, improves the strength of the welded joints, ensures continuous and stable production of nickel-copper alloy rolls, and reduces the risk of broken belts in the production line.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a continuous production method for an annealing and pickling line of a nickel-copper alloy coiled plate. The continuous production method comprises the following steps: (1) preparing protective gas and adjusting the flow; (2) selecting a connecting material and a filler wire material; (3) preparing a groove; (4) automatic welding is conducted through an MAG welding machine; and (5) cutting a crescent on a welding seam. And a nickel-copper alloy coiled plate finished product is obtained according to a continuous annealing and pickling line conventional process subsequently. According to the method, when a stainless steel continuous annealing and pickling line is used for welding the nickel-copper alloy coiled plates including Monel 400, by selecting reasonable connecting materials and welding wires and reasonably controlling welding parameters, liquefaction cracks of welding joints are effectively avoided, the strength of the welding joints is guaranteed, and continuous and stable production of the nickel-copper alloy coiled plates is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nickel-copper alloy welding, in particular to a continuous production method of a nickel-copper alloy coil annealing and pickling line. Background Art

[0002] Monel 400 alloy is a nickel-copper corrosion-resistant alloy with excellent corrosion resistance and oxidation resistance, as well as high comprehensive mechanical properties. It is widely used in energy, petrochemical, marine, aerospace and other fields. Wide-width nickel-copper alloy products (≥1030mm) are generally produced by stainless steel coil production lines. When Monel 400 alloy is produced in the stainless steel annealing and pickling line, it is necessary to weld the Monel 400 alloy coil with the connecting material through a MAG welder to achieve continuous production. Monel 400 alloy has a high Cu content (≥30%), and Cu tends to infiltrate the austenite grain boundary in stainless steel, so the welded joint is prone to serious liquefaction cracking problems. The commonly used connecting materials for stainless steel production lines are 304 austenitic stainless steel and the filler wire is ER309L-Si stainless steel welding wire. When Monel 400 alloy uses conventional stainless steel welding technology, the weld pool will be enriched with Cu elements due to the dilution effect of the base material Monel400, forming a large number of liquefaction cracks, and the weld quality is unqualified, resulting in the inability to achieve continuous production. In addition, nickel-based alloys have poor fluidity and wettability in liquid state, and cracks and pores are very likely to occur during welding. The above characteristics make Monel 400 alloy extremely difficult to weld in the production of stainless steel continuous annealing and pickling lines, and it is very easy to cause weld cracks and lead to vicious production accidents such as broken belts on the production line. Summary of the invention

[0003] Based on the above, in order to solve the technical problem that the existing nickel-copper alloy is extremely difficult to weld during the production of stainless steel continuous annealing and pickling lines, and is prone to weld cracking, resulting in vicious production accidents such as broken belts on the production line, the purpose of the present invention is to provide a nickel-copper alloy coil annealing and pickling line continuous production method to achieve continuous and stable production of nickel-copper alloy in stainless steel hot annealing and pickling lines.

[0004] To achieve its purpose, the present invention adopts the following technical solution: A continuous production method for a nickel-copper alloy coil annealing and pickling line comprises the following steps: Step 1: Prepare protective gas and adjust flow rate Use argon-oxygen mixed gas as shielding gas to protect the weld; Step 2: Selection of connecting materials and filler wire materials The connecting material is 304 austenitic stainless steel coil or N6 pure nickel coil with a thickness close to that of nickel-copper alloy: when the connecting material is 304 austenitic stainless steel coil, the welding wire is ERNiCrMo-3; when the connecting material is N6 pure nickel coil, the welding wire is ER309L-Si stainless steel welding wire; Step 3: Bevel preparation The nickel-copper alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding with MAG welding machine When ERNiCrMo-3 welding wire is selected, the welding parameters are controlled as follows: weld gap 1.8~2.2mm, welding voltage 26~28V, wire feeding speed 11~12m / min, welding speed 0.7~0.8m / min, welding torch height 15~17mm, and the welding gun is adjusted to the base material on the 304 austenitic stainless steel coil side; When ER309L-Si welding wire is selected, the welding parameters are controlled as follows: weld gap 1.6~2.0mm, welding voltage 25~27V, wire feeding speed 12~13m / min, welding speed 0.7~0.9m / min, welding torch height 19~21mm, and the welding gun is adjusted to be biased towards the base material of the N6 pure nickel coil side; Step 5: Cut the crescent of the weld Cut the crescent at the arc starting and arc ending parts of the weld, and then follow the conventional process of continuous annealing and pickling line to obtain nickel-copper alloy coils. Finished product.

[0005] As a further preferred embodiment of the technical solution of the present invention, the width of the nickel-copper alloy is ≥1030 mm. Preferably, the nickel-copper alloy is Monel 400 nickel-copper corrosion-resistant alloy.

[0006] Furthermore, the Monel 400 nickel-copper corrosion-resistant alloy has a thickness of 3.0-6.0 mm.

[0007] Furthermore, in step 1, the argon-oxygen mixed gas is a mixture of Ar and 1-2% by volume of O2. Adding a small amount of active gas O2 (1-2%) to the shielding gas can improve the quality of weld formation.

[0008] Furthermore, in step 1, the flow rate of the argon-oxygen mixed gas is 13-15 L / min. Since the thickness of the base material is 3.0-6.0 mm, a flow rate that is too low (<13 L / min) will not achieve the effect of protecting the weld, and a flow rate that is too high (>15 L / min) will increase the consumption of argon gas and may also cause spattering of the weld material.

[0009] During the continuous production of the annealing and pickling line, the weld joints have defects such as liquefaction cracks and pores, which are very likely to cause weld cracking and lead to malignant production accidents such as belt breakage on the production line. The present invention proposes a new continuous production process, which has the following beneficial effects compared with the traditional process: When welding nickel-copper alloy coils including Monel 400 using a stainless steel continuous annealing and pickling line, the liquefaction cracks of the welded joints are effectively avoided by selecting reasonable connecting materials and welding wires, and by reasonably controlling the welding parameters, the strength of the welded joints is ensured, ensuring the continuous and stable production of nickel-copper alloy coils. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is a low-magnification photograph of liquefaction cracks in the welded joint of Monel 400 alloy using conventional welding technology; Figure 2 This is a metallographic photograph of liquefaction cracks in the welded joint of Monel 400 alloy using conventional welding technology; Figure 3 This is a low magnification photo of the welded joint in Example 1 of the present invention. Figure 4 These are photos of the weld face bend and back bend in Example 1 of the present invention. DETAILED DESCRIPTION

[0011] The present invention is further described below by means of specific embodiments in conjunction with the accompanying drawings, but the present invention is not limited in any form.

[0012] The present invention takes Monel 400 as an example to describe in detail the continuous production method of the nickel-copper alloy coil annealing and pickling line.

[0013] Figure 1 The low-power photo of the liquefaction crack of the welded joint of Monel 400 alloy using conventional welding technology is shown in Figure 1 , metallographic photos see Figure 2 The method of the present invention is described in the following examples.

[0014] Example 1 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 6.0mm: Step 1: Prepare protective gas and adjust flow rate Ar+2%O2 is used to protect the weld, and the protective gas flow rate is 15L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 6.0mm thick 304 austenitic stainless steel coil, and the welding wire material is ERNiCrMo-3 nickel-based welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 2.2mm, the welding voltage is 28V, the wire feeding speed is 12m / min, the welding speed is 0.7m / min, the welding torch height is 15mm, and the welding torch is adjusted to the base material on the 304 austenitic stainless steel coil side; Step 5: Cut the crescent of the weld Cut the crescent at the arc starting and arc ending parts of the weld. Figure 3 ) No cracks, weld face bend and back bend ( Figure 4 ) are intact, and subsequently the conventional process of continuous annealing and pickling line is followed to obtain the finished nickel-copper alloy coil.

[0015] Example 2 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 3.0mm: Step 1: Prepare protective gas and adjust flow rate Ar+2%O2 is used to protect the weld, and the protective gas flow rate is 13L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 304 austenitic stainless steel coil with a thickness of 3.0 mm, and the welding wire material is ERNiCrMo-3 nickel-based welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 1.8mm, the welding voltage is 26V, the wire feeding speed is 11m / min, the welding speed is 0.8m / min, the welding torch height is 17mm, and the welding torch is adjusted to the base material on the 304 austenitic stainless steel coil side; Step 5: Cut the crescent of the weld Crescents are cut on the arc starting and ending parts of the weld, and the weld face bend and back bend are intact. Subsequently, the nickel-copper alloy coil product is obtained according to the conventional process of the continuous annealing and pickling line.

[0016] Example 3 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 4.0mm: Step 1: Prepare protective gas and adjust flow rate Ar+2%O2 is used to protect the weld, and the protective gas flow rate is 14L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 4.0mm thick 304 austenitic stainless steel coil, and the welding wire material is ERNiCrMo-3 nickel-based welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 2.0 mm, the welding voltage is 27 V, the wire feeding speed is 11.5 m / min, the welding speed is 0.75 m / min, the welding torch height is 16 mm, and the welding torch is adjusted to the base material on the 304 austenitic stainless steel coil side; Step 5: Cut the crescent of the weld Crescents are cut on the arc starting and ending parts of the weld, and the weld face bend and back bend are intact. Subsequently, the nickel-copper alloy coil product is obtained according to the conventional process of the continuous annealing and pickling line.

[0017] Example 4 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 6.0mm: Step 1: Prepare protective gas and adjust flow rate Ar+1%O2 is used to protect the weld, and the protective gas flow rate is 15L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 6.0mm thick N6 pure nickel coil, and the welding wire material is ER309L-Si stainless steel welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 2.2mm, the welding voltage is 28V, the wire feeding speed is 12m / min, the welding speed is 0.7m / min, the welding torch height is 15mm, and the welding gun is adjusted to be biased towards the N6 pure nickel coil; Step 5: Cut the crescent of the weld The arc starting and arc ending parts of the weld are cut into crescents, and the weld face bend and back bend are intact. Subsequently, the nickel-copper alloy coil is obtained according to the conventional process of the continuous annealing and pickling line.

[0018] Example 5 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 3.0mm: Step 1: Prepare protective gas and adjust flow rate Ar+1%O2 is used to protect the weld, and the protective gas flow rate is 14L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 3.0mm thick N6 pure nickel coil, and the welding wire material is ER309L-Si stainless steel welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 1.8mm, the welding voltage is 26V, the wire feeding speed is 11m / min, the welding speed is 0.8m / min, the welding torch height is 17mm, and the welding gun is adjusted to be biased towards the N6 pure nickel coil; Step 5: Cut the crescent of the weld The arc starting and arc ending parts of the weld are cut into crescents, and the weld face bend and back bend are intact. Subsequently, the nickel-copper alloy coil is obtained according to the conventional process of the continuous annealing and pickling line.

[0019] Example 6 Continuous production method of Monel 400 alloy coil continuous annealing and pickling line with a thickness of 4.0mm: Step 1: Prepare protective gas and adjust flow rate The shielding gas uses Ar+1%O2 to protect the weld, and the shielding gas flow rate is 13L / min; Step 2: Selection of connecting materials and filler wire materials The connection material is 4.0mm thick N6 pure nickel coil, and the welding wire material is ER309L-Si stainless steel welding wire; Step 3: Bevel preparation Use a shearing device to shear the Monel 400 coil to be welded into an I-type groove; Step 4: Automatic welding with MAG welding machine The weld gap is 2.0mm, the welding voltage is 27V, the wire feeding speed is 11.5m / min, the welding speed is 0.75m / min, the welding torch height is 16mm, and the welding gun is adjusted to be biased towards the N6 pure nickel coil; Step 5: Cut the crescent of the weld The arc starting and arc ending parts of the weld are cut into crescents, and the weld face bend and back bend are intact. Subsequently, the nickel-copper alloy coil is obtained according to the conventional process of the continuous annealing and pickling line.

Claims

1. A continuous production method for a nickel-copper alloy coil annealing and pickling line, It is characterized in that The following steps are involved: Step 1: Prepare protective gas and adjust flow rate Use argon-oxygen mixed gas as shielding gas to protect the weld; Step 2: Selection of connecting materials and filler wire materials The connecting material is 304 austenitic stainless steel coil or N6 pure nickel coil with a thickness close to that of nickel-copper alloy: when the connecting material is 304 austenitic stainless steel coil, the welding wire is ERNiCrMo-3; when the connecting material is N6 pure nickel coil, the welding wire is ER309L-Si stainless steel welding wire; Step 3: Bevel preparation The nickel-copper alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding with MAG welding machine When ERNiCrMo-3 welding wire is selected, the welding parameters are controlled as follows: weld gap 1.8~2.2mm, welding voltage 26~28V, wire feeding speed 11~12m / min, welding speed 0.7~0.8m / min, welding torch height 15~17mm, and the welding gun is adjusted to the base material on the 304 austenitic stainless steel coil side; When ER309L-Si welding wire is selected, the welding parameters are controlled as follows: weld gap 1.6~2.0mm, welding voltage 25~27V, wire feeding speed 12~13m / min, welding speed 0.7~0.9m / min, welding torch height 19~21mm, and the welding gun is adjusted to be biased towards the base material of the N6 pure nickel coil side; Step 5: Cut the crescent of the weld Cut the crescent at the arc starting and arc ending parts of the weld, and then follow the conventional process of continuous annealing and pickling line to obtain nickel-copper alloy coils. Finished product.

2. A continuous production method for a nickel-copper alloy coil annealing and pickling line as claimed in claim 1, It is characterized in that The width of the nickel-copper alloy is ≥1030 mm.

3. A continuous production method for annealing and pickling line of nickel-copper alloy coils as claimed in claim 3, It is characterized in that The nickel-copper alloy is Monel 400 nickel-copper corrosion-resistant alloy.

4. A continuous production method for a nickel-copper alloy coil annealing and pickling line as claimed in claim 4, It is characterized in that The Monel 400 nickel-copper corrosion-resistant alloy has a thickness of 3.0-6.0 mm.

5. A continuous production method for a nickel-copper alloy coil annealing and pickling line as claimed in any one of claims 1 to 4, It is characterized in that In step 1, the argon-oxygen mixed gas is Ar and O with a volume fraction of 1-2%. 2 mixture.

6. A continuous production method for annealing and pickling line of nickel-copper alloy coils as claimed in claim 5, It is characterized in that In step 1, the flow rate of the argon-oxygen mixed gas is 13-15 L / min.