Carbon-carbon composite crucible side preform and preparation method thereof
By using vertical wire wound, mesh timber laying and needle-punching, ring wire winding, mesh wisting, mesh wisting and arc-segregation processes in the production of carbon-carbon composite pots, the problem of carbon wire damage is solved and improved The mechanical strength and service life of the carbon-carbon composite cauldron prefabricated body.
Patent Information
- Application Number
- CN202411151914.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
AI Technical Summary
During the production process of traditional carbon carbon cauldron prefabricated carbon filaments, carbon filaments are easily damaged during textile and needle puncture, resulting in a decrease in strength and affecting the internal structure and service life of the crucible.
The methods of vertical wire winding, mesh tire laying and needle-punching, ring wire winding, mesh wire winding and arc segment thickening are adopted to reduce carbon wire damage and form a carbon-carbon composite cauldron prefabricated body with high overall mechanical strength.
It effectively reduces the damage of carbon filaments, improves the internal structural integrity and mechanical strength of the carbon-carbon composite prefabricated body, and improves the performance and life.
Smart Images

Figure BDA0005003879570000061 
Figure HDA0005003879580000011 
Figure HDA0005003879580000021
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of a brazed preform, and in particular to a carbon-carbon composite brazed preform and a preparation method thereof. Background Art
[0002] Carbon-carbon composite materials are widely used in aerospace, metallurgy, chemical industry and other fields due to their excellent high temperature performance, mechanical properties and thermal properties. As an important component of the crucible, the performance of the crucible directly affects the service life and effect of the crucible.
[0003] The traditional production method of carbon-carbon braided preforms is to use carbon fiber filaments to weave into carbon cloth and mesh respectively, and then strengthen the internal structure by needle punching and winding, so as to weave into a preform; however, in the process of weaving the above carbon fiber filaments, since the carbon filaments will alternate in warp and weft, the mechanical equipment will damage the strength of the carbon filaments during the production process, so that after the T700-level carbon filaments are processed by weaving, the strength of the carbon filaments will be reduced from the original 4900MPa to about 3500MPa, and the strength of the carbon filaments with lower strength will be reduced to even lower after needle punching, which will have a great impact on the internal structure, overall mechanical strength and later service life of the braided preform.
[0004] Therefore, it is necessary to provide a method for preparing a carbon-carbon composite brass preform to reduce damage to the carbon filaments, improve the internal structure and overall mechanical strength of the carbon-carbon composite brass preform, thereby improving the performance of the carbon-carbon composite brass preform and extending its service life. Summary of the invention
[0005] In order to reduce carbon filament damage, improve the internal structure of a carbon-carbon composite crucible preform, and enhance the overall mechanical strength, the present application provides a carbon-carbon composite crucible preform and a preparation method thereof.
[0006] The preparation method of the carbon-carbon fiber composite braided preform provided in the present application adopts the following technical scheme: A method for preparing a carbon-carbon fiber composite braided preform comprises the following steps: S1. Vertical winding: set the mold and arrange the upper and lower iron nails according to the preset size of the carbon-carbon composite braided preform, and use carbon wire to vertically connect the upper and lower iron nails to form a vertical fiber layer; the vertical winding density is 18.5-22.5 wires / 10cm; S2. Laying of mesh and needling: Laying of mesh on the surface of the vertical fiber layer and then needling; S3, hoop winding: use carbon filaments to hoop winding on the surface of the mesh after S2 needle punching to form a hoop fiber layer; the hoop winding density is 18.5-22.5 strands / 10cm; S4, mesh laying and needling: laying the mesh on the surface of the circumferential fiber layer, and then needling; S5, grid winding: pull the carbon filament obliquely from the end of the straight section of the mold to the bottom of the mold, pull it horizontally on the bottom platform and then pull it back obliquely to the end of the straight section, repeat the operation to achieve grid winding; S6, S1 to S5 form a unit layer, and the above S1 to S5 are repeated 4 times until the fifth unit layer is completed; S7, then repeat the arc segment thickening and unit layer laying until the required thickness is reached to obtain a carbon-carbon composite brass preform.
[0007] In a specific embodiment, the vertical winding density and the hoop winding density can also be 18.5 wires / 10cm or 22.5 wires / 10cm.
[0008] Optionally, in step S5, the carbon filament is pulled obliquely from the end of the straight section of the mold to the bottom of the mold at a rotation angle of 135°±10°, and after being pulled horizontally and rotated, the carbon filament is pulled obliquely back to the end of the straight section at a rotation angle of 35°±10°.
[0009] Optionally, in steps S2 and S4, the weight ratio of the web to the vertical fiber layer or the circumferential fiber layer is 1:(5-7).
[0010] Optionally, in steps S2 and S4, the weight ratio of the web to the vertical fiber layer or the circumferential fiber layer is 1:(5.5-6.5).
[0011] In some embodiments, the weight ratio of the mesh to the vertical fiber layer or the circumferential fiber layer can be 1:(5-5.5), 1:(5-6), 1:(5-6.5), 1:(5-7), 1:(5.5-6), 1:(5.5-6.5), 1:(5.5-7), 1:(6-6.5), 1:(6-7) or 1:(6.5-7).
[0012] In a specific embodiment, the weight ratio of the web to the vertical fiber layer or the hoop fiber layer may also be 1:5, 1:5.5, 1:6, 1:6.5 or 1:7.
[0013] Optionally, in step S5, the carbon filament spacing of the grid winding is 25-40 mm.
[0014] In some embodiments, the carbon filament spacing of the grid winding may be 25-30 mm, 25-35 mm, 25-40 mm, 25-45 mm, 30-35 mm, 30-40 mm, 30-45 mm, 35-40 mm, 35-45 mm, or 40-45 mm.
[0015] Optionally, the carbon filament spacing of the grid winding may also be 25 mm, 30 mm, 35 mm, 40 mm or 45 mm.
[0016] Optionally, the specific steps of the arc segment thickening are: cutting the carbon fiber filaments into bundles that match the circumference length of the arc segment at the R corner, laying the cut bundles flatly at the R corner, and fixing them with a mesh; laying a layer of mesh on the surface of the bundles laid at the R corner and then performing acupuncture.
[0017] Optionally, the acupuncture adopts a needle arrangement method with a needle spacing of 5 mm, and the thickness of the acupuncture is 15-16 cm.
[0018] In a second aspect, the present application provides a carbon-carbon composite brass preform.
[0019] A carbon-carbon composite crucible preform is prepared by adopting the method for preparing the carbon-carbon composite crucible preform.
[0020] Optionally, the carbon-carbon composite brass preform has an outer diameter of 993±2 cm, an inner diameter of 941±2 cm, a total length of 649±2 cm, and a straight section length of 549±2 cm.
[0021] In summary, this application has the following beneficial effects: 1. The present application provides a method for preparing a carbon-carbon composite Crusher preform, which comprises the steps of vertical wire winding, mesh laying and needling, circumferential wire winding, mesh laying and needling, grid wire winding and arc segment thickening. The carbon-carbon composite Crusher preform is prepared by the above method, which can effectively reduce the damage to the carbon wire during the processing, improve the internal defects and structural integrity of the carbon-carbon composite Crusher preform, thereby obtaining a carbon-carbon composite Crusher preform with excellent overall mechanical strength.
[0022] 2. The volume density of the carbon-carbon composite brazed preform obtained in this application is 0.45-0.48 g / cm 3 The tensile strength in the X direction is 5.28-6.21MPa, the tensile strength in the Y direction is 5.61-6.51MPa, and the tensile strength in the Z direction is 2.25-2.43MPa.
[0023] 3. The present application further controls the weight ratio of the mesh to the vertical fiber layer or the circumferential fiber layer within the range of 1: (5.5-6.5), and the carbon filament spacing of the mesh winding is controlled within the range of 25-40 mm. The obtained carbon-carbon composite braided preform is more uniform and has a higher overall mechanical strength. Its volume density is 0.46-0.48 g / cm 3 The tensile strength in the X direction is 5.28-6.21MPa, the tensile strength in the Y direction is 5.61-6.51MPa, and the tensile strength in the Z direction is 2.25-2.43MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a flow chart of the preparation method of the carbon-carbon crucible preform provided in the present application; Figure 2 It is a preset size mold for the carbon-carbon composite crucible preform used in this application; Figure 3 It is a schematic diagram of the structural dimensions of the carbon-carbon crucible preform provided in this application. DETAILED DESCRIPTION
[0025] The present application provides a method for preparing a carbon-carbon braided preform, comprising the following steps: S1. Vertical winding: Set the mold according to the preset size of the carbon-carbon composite crucible preform (such as Figure 1 As shown, the mold is made of solid wood, the outer surface is wrapped with aluminum-plastic panels, and iron nails are arranged on the upper and lower bottom edges of the mold); carbon wires are used to vertically connect the upper and lower iron nails to form a vertical fiber layer; the vertical winding density is 18.5-22.5 wires / 10cm.
[0026] S2. Laying of mesh and needling: Lay the mesh on the surface of the vertical fiber layer, and then use a 5mm needle spacing method to needle punch; the weight ratio of the mesh to the vertical fiber layer is 1: (5-7), and the needling thickness is 15-16cm; further, the weight ratio of the mesh to the vertical fiber layer is 1: (5.5-6.5).
[0027] S3, hoop winding: use carbon filaments to carry out hoop winding on the surface of the mesh after S2 needle punching to form a hoop fiber layer; the density of the hoop winding is 18.5-22.5 strands / 10cm.
[0028] S4, mesh laying and needling: the mesh is laid on the surface after the circumferential winding, and then acupuncture is performed using a 5mm needle spacing method; the weight ratio of the mesh to the circumferential fiber layer is 1: (5-7), and the needling thickness is 15-16cm. Furthermore, the weight ratio of the mesh to the circumferential fiber layer is 1: (5.5-6.5).
[0029] S5. Grid winding: pull the carbon filament obliquely 135° from the end of the straight section of the mold and rotate it to the bottom of the mold. Pull it horizontally 35° on the bottom platform and rotate it, then pull it obliquely back to the end of the straight section. Repeat the operation to achieve grid winding. The carbon filament spacing of the grid winding is 25-45mm; further, the carbon filament spacing of the grid winding is 25-40mm.
[0030] S6, continue to repeat the above steps S1 to S5 4 times (steps S1 to S5 complete a unit layer), until the fifth unit layer is completed; S7. Use a contour ruler to locate the position that needs to be thickened; cut the carbon fiber yarn into a tow that meets the perimeter length of the R corner, lay the cut tow evenly at the R corner, and fix it with a mesh tire; lay a layer of mesh tire on the surface of the tow at the R corner and then perform acupuncture to achieve arc segment thickening; S8, then lay one more unit layer (steps S1 to S5), thicken the arc segment once (step S7), lay one more unit layer (steps S1 to S5), thicken the arc segment once (step S7)... and repeat this process until the desired thickness is reached (the total number of unit layers is approximately 30±2 layers), thereby obtaining a carbon-carbon composite brazed preform.
[0031] In the embodiment of the present application, the model of the carbon filament is T700-12K, and the strength is 4900MPa; the mesh tire is made of T700-12K carbon filament, and the mass density is 50g / m 2 The remaining raw materials, reagents, solvents, etc. can be obtained commercially.
[0032] The present application is further described in detail below in combination with embodiments, performance testing and accompanying drawings.
[0033] Example 1 Example 1 provides a method for preparing a carbon-carbon composite brass preform.
[0034] The method for preparing the carbon-carbon composite brazed preform comprises the following steps: S1. Vertical winding: Set the mold and arrange the upper and lower iron nails according to the preset size of the carbon-carbon composite braided preform, and use carbon wire to connect vertically between the upper and lower iron nails to form a vertical fiber layer; the vertical winding density is 18.5 wires / 10cm (instead of 300g / m 2 of carbon cloth).
[0035] S2. Laying of mesh and needling: Lay the mesh on the surface of the vertical fiber layer, and then use a 5mm needle spacing method to perform needling; the weight ratio of the mesh to the vertical fiber layer is 1:6, and the needling thickness is 15-16cm.
[0036] S3, hoop winding: use carbon filaments to carry out hoop winding on the surface of the web after S2 needle punching to form a hoop fiber layer; the density of the hoop winding is 18.5 strands / 10cm.
[0037] S4. Laying of mesh and needling: Lay the mesh on the surface after the hoop winding, and then use a 5mm needle spacing method to perform needling; the weight ratio of the mesh to the hoop fiber layer is 1:6, and the needling thickness is 15-16cm.
[0038] S5, grid winding: pull the carbon filament obliquely 135° from the end of the straight section of the mold to the bottom of the mold, pull it horizontally 35° on the bottom platform, rotate it, and then pull it obliquely back to the end of the straight section. Repeat the operation to achieve grid winding. The carbon filament spacing of the grid winding is 35mm.
[0039] S6, continue to repeat the above steps S1 to S5 4 times (steps S1 to S5 complete a unit layer), until the fifth unit layer is completed; S7. Use a contour ruler to locate the position that needs to be thickened; cut the carbon fiber yarn into a tow that meets the perimeter length of the R corner, lay the cut tow evenly at the R corner, and fix it with a mesh tire; lay a layer of mesh tire on the surface of the tow at the R corner and then perform acupuncture to achieve arc segment thickening; S8, and then lay a unit layer (steps S1 to S5), thicken the arc segment once (step S7), lay a unit layer (steps S1 to S5), thicken the arc segment once (step S7)..., repeat this process until the required thickness is reached (the total number of unit layers is about 30 layers), and a carbon-carbon composite Zhanbang preform is obtained. The carbon-carbon composite Zhanbang preform has an outer diameter of 993±2cm, an inner diameter of 941±2cm, a total length of 649±2cm, and a straight section length of 549±2cm.
[0040] Embodiment 2-5 Examples 2-5 respectively provide a method for preparing a carbon-carbon composite brass preform.
[0041] The difference between the above embodiment and embodiment 1 is that the weight ratio of the web and the vertical fiber layer or the circumferential fiber layer in steps S2 and S4 is specifically shown in Table 1 below.
[0042] Table 1 Weight ratio of the web and the vertical fiber layer or the hoop fiber layer in the preparation method of Examples 1-5 Example Weight ratio of the web to the vertical fiber layer or the hoop fiber layer 1 1:6 2 1:5 3 1:5.5 4 1:6.5 5 1:7 Embodiment 6-9 Examples 6-9 respectively provide a method for preparing a carbon-carbon composite brass preform.
[0043] The difference between the above embodiment and embodiment 1 is that: S5, the carbon filament spacing of the grid winding in the grid winding step is specifically shown in Table 2 below.
[0044] Table 2 Carbon filament spacing of mesh winding in Example 1, Example 6-9 Example Carbon filament spacing of mesh winding (mm) 1 35 6 25 7 30 8 40 9 45 Example 10 Example 10 provides a method for preparing a carbon-carbon composite brass preform.
[0045] The difference between the above embodiment and embodiment 1 is that the vertical winding density in the vertical winding step S1 is 22.5 strands / 10cm, and the hoop winding density in the hoop winding step S3 is 22.5 strands / 10cm. (Instead of 360g / m 2 Carbon cloth. ) Performance test The carbon-carbon composite Zhuobang preforms obtained in Examples 1-10 and commercially available Zhuobang preforms were tested for product density and mechanical properties. The results are shown in Table 3 below.
[0046] (1) Product density detection method: Take three 1 cm thick samples from different parts (R corners, straight sections) along the inner, middle and outer directions of the preform that has been completed and solidified. 3 The volume density of the prefabricated cube is measured, and the density difference is required to be no greater than 0.01g / cm 3 ; (2) Tensile strength test method: Take three small strips (length × width × height of 150 mm × 20 mm × 10 mm) from the straight section of the carbon-carbon composite braided preform in the circumferential direction and the perpendicular circumferential direction for tensile strength test. The tensile strength test method refers to GB_T 3362-2017 Carbon fiber multifilament tensile performance test method.
[0047] Note: The commercially available Brass preform uses carbon filaments as the raw material for weaving, and is woven into carbon cloth according to the standard of warp and weft density of 18.5 strands / 10cm or 22.5 strands / 10cm. The following tests use two commercially available Brass preform models: The weft density of commercially available product ① is 18.5 strands / 10cm, and the dimensions are: outer diameter φ993mm×inner diameter φ941mm×height 599mm. The weft density of commercially available product ② is 22.5 strands / 10cm, and the dimensions are: outer diameter φ993mm×inner diameter φ941mm×height 549mm.
[0048] Table 3 Tensile test results of carbon-carbon composite brass preforms of Examples 1-10 and Comparative Example 1 According to the test results in Table 3, the volume density of the carbon-carbon composite brazed preform obtained in Examples 1-9 of the present application is 0.45-0.48 g / cm 3, the tensile strength in the X direction is 5.28-6.21MPa, the tensile strength in the Y direction is 5.61-6.51MPa, and the tensile strength in the Z direction is 2.25-2.43MPa; while the tensile strength in the X direction of the commercially available product ① is only 4.31MPa, the tensile strength in the Y direction is only 4.26MPa, and the tensile strength in the Z direction is only 1.59MPa. The tensile strength in the X direction of the carbon-carbon composite brass preform obtained in Example 10 is 6.27MPa, the tensile strength in the Y direction is 6.59MPa, and the tensile strength in the Z direction is 3.22MPa; while the tensile strength in the X direction of the commercially available product ② is only 5.43MPa, the tensile strength in the Y direction is only 5.15MPa, and the tensile strength in the Z direction is only 1.66MPa. Therefore, it is explained that the carbon-carbon composite brazed preform prepared by vertical wire winding, mesh laying and needling, hoop wire winding, grid wire winding and thickening processes in the present application has the advantages of good structural integrity, uniform volume density, and excellent overall mechanical strength in X, Y and Z directions.
[0049] From the test results of Examples 1-5, it can be seen that when the weight ratio of the mesh to the vertical fiber layer or the circumferential fiber layer in Examples 2 and 5 is controlled to 1:5 or 1:7, the tensile strength of the obtained carbon-carbon composite brass preform in the X direction is 5.28-5.45MPa, the tensile strength in the Y direction is 5.61-5.78MPa, and the tensile strength in the Z direction is 2.25-2.30MPa; and when the weight ratio of the mesh to the vertical fiber layer or the circumferential fiber layer in Examples 1 and 3-4 is controlled to 1:(5.5-6.5), the tensile strength of the obtained carbon-carbon composite brass preform in the X direction is 5.87-6.14MPa (≥5.50MPa), the tensile strength in the Y direction is 6.17-6.43MPa (≥6.00MPa), and the tensile strength in the Z direction is 2.31-2.38MPa (≥2.30MPa). Therefore, it is explained that the present application further controls the weight ratio of the web to the vertical fiber layer or the circumferential fiber layer within the range of 1:(5.5-6.5), and the overall mechanical strength of the obtained carbon-carbon composite brazed preform is more excellent.
[0050] The test results of Example 1 and Examples 6-9 show that as the carbon filament spacing of the mesh winding increases in the mesh winding step, the volume density of the obtained carbon-carbon composite brass preform gradually decreases, and the overall mechanical strength also gradually decreases; further comparison shows that when the carbon filament spacing of the mesh winding is controlled at 45 mm in Example 9, the volume density of the obtained carbon-carbon composite brass preform is only 0.45 g / cm 3 When the carbon wire spacing of the mesh winding is controlled at 30-40 mm in Examples 1 and 6-8, the volume density of the obtained carbon-carbon composite preform is 0.46-0.47 g / cm 3 (>0.45g / cm3 ), and the tensile strength in the X direction is 6.09-6.18MPa (>6.00MPa), the tensile strength in the Y direction is 6.35-6.48MPa (>6.00MPa), and the tensile strength in the Z direction is 2.32-2.40MPa (>2.30MPa). Therefore, it is explained that the present application further controls the carbon filament spacing of the mesh winding in the mesh winding step within the range of 30-40mm, and the obtained carbon-carbon composite brass preform is more uniform and has a higher overall mechanical strength.
[0051] In summary, the present application provides a method for preparing a carbon-carbon composite braided preform, which prepares a carbon-carbon composite braided preform with good uniformity and excellent mechanical strength by adopting the steps of vertical winding, mesh laying and needle punching, hoop winding, mesh winding and thickening. The present application further controls the weight ratio of the mesh to the vertical fiber layer or the hoop fiber layer within the range of 1: (5.5-6.5), and the carbon filament spacing of the mesh winding within the range of 30-40 mm, so that the obtained carbon-carbon composite braided preform is more uniform and has higher overall mechanical strength.
[0052] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements made without departing from the spirit of the present invention are within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a carbon-carbon composite brass preform, characterized in that: The following steps are involved: S1. Vertical winding: set the mold and arrange the upper and lower iron nails according to the preset size of the carbon-carbon composite braided preform, and use carbon wire to vertically connect the upper and lower iron nails to form a vertical fiber layer; the vertical winding density is 18.5-22.5 wires / 10cm; S2. Laying of mesh and needling: Laying of mesh on the surface of the vertical fiber layer and then needling; S3, hoop winding: use carbon filaments to hoop winding on the surface of the mesh after S2 needle punching to form a hoop fiber layer; the hoop winding density is 18.5-22.5 strands / 10cm; S4, mesh laying and needling: laying the mesh on the surface of the circumferential fiber layer, and then needling; S5, grid winding: pull the carbon filament obliquely from the end of the straight section of the mold to the bottom of the mold, pull it horizontally on the bottom platform and then pull it obliquely back to the end of the straight section, repeat the operation to achieve grid winding; S6, S1-S5 form a unit layer, and the above S1-S5 are repeated 4 times until the fifth unit layer is completed; S7, then repeat the arc segment thickening and unit layer laying until the required thickness is reached to obtain a carbon-carbon composite brass preform.
2. The method for preparing a carbon-carbon composite braided preform according to claim 1, characterized in that: In the steps S2 and S4, the weight ratio of the web to the vertical fiber layer or the circumferential fiber layer is 1:(5-7).
3. The method for preparing a carbon-carbon composite braided preform according to claim 1, characterized in that: In the steps S2 and S4, the weight ratio of the web to the vertical fiber layer or the circumferential fiber layer is 1:(5.5-6.5).
4. The method for preparing a carbon-carbon composite braided preform according to claim 1, characterized in that: In the step S5, the carbon filament spacing of the grid winding is 25-40 mm.
5. The method for preparing a carbon-carbon composite braided preform according to any one of claims 1 to 4, characterized in that: The specific steps of the arc segment thickening are: cutting the carbon fiber filaments into bundles that meet the circumference length of the arc segment R corner, laying the cut bundles flatly at the R corner, and fixing them with a mesh; laying a layer of mesh on the surface of the bundles laid at the R corner and then performing acupuncture.
6. The method for preparing a carbon-carbon composite braided preform according to claim 1, characterized in that: The acupuncture adopts a needle arrangement method with a needle spacing of 5 mm, and the thickness of the acupuncture is 15-16 cm.
7. A carbon-carbon composite Crushing preform prepared by the method for preparing a carbon-carbon composite Crushing preform according to any one of claims 1 to 6.
8. The carbon-carbon composite braided preform according to claim 7, characterized in that: The carbon-carbon composite brass preform has an outer diameter of 993±2 cm, an inner diameter of 941±2 cm, a total length of 649±2 cm, and a straight section length of 549±2 cm.
Citation Information
Cited By
Intelligent control method and system for twining thorns on crucible
CN120949567A