Doped and coated high-nickel positive electrode material as well as preparation method and application thereof

By using spray pyrolysis and cerium oxide coating, the problems of capacity decay and poor thermal stability of high-nickel cathode materials during cycling were solved. This approach achieved uniform doping of the material and simplified the process, thereby improving the stability and performance of the material.

CN118877950APending Publication Date: 2024-11-01JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410885804.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing high-nickel cathode materials suffer from capacity decay and poor thermal stability during cycling, and their preparation process is complex and generates a large amount of wastewater.

Method used

A method for preparing aluminum doping and cerium oxide coating using spray pyrolysis is proposed. The spray pyrolysis method achieves uniform distribution of aluminum in high-nickel materials, and the cerium oxide coating improves the cycling performance and thermal stability of the materials.

Benefits of technology

It effectively reduces the degree of Li/Ni mixing, improves the cycle stability and rate performance of the cathode material, simplifies the preparation process, reduces wastewater generation, and lowers production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926019260000111
    Figure BDA0004926019260000111
Patent Text Reader

Abstract

The invention provides a doped and coated high-nickel positive electrode material as well as a preparation method and application thereof. The preparation method comprises the following steps: performing spray pyrolysis on a nickel-cobalt-manganese-aluminum mixed salt solution to obtain a nickel-cobalt-manganese-aluminum precursor; and mixing the nickel-cobalt-manganese-aluminum precursor, a lithium source and a cerium source, and sintering to obtain the doped and coated high-nickel positive electrode material, wherein the total molar weight of nickel, cobalt and manganese is 100%, and the molar ratio of nickel is larger than or equal to 80%. According to the preparation method provided by the invention, through a spray pyrolysis method, uniform distribution of aluminum in the high-nickel material is realized, generation of an aluminum segregation phenomenon is avoided, and the cycle performance, the conductivity and the thermal stability of the material are effectively improved by cooperating with coating of cerium dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries and relates to a doped and coated high-nickel positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries play an important role in new energy vehicles, electronic products and energy storage due to their advantages such as high energy density, low cost and long cycle life. Currently, the common positive electrode materials for lithium batteries are mainly lithium cobalt oxide, lithium iron phosphate and ternary materials (lithium nickel cobalt manganese oxide, etc.). Among them, high nickel layered positive electrode material LiNi x Co y Mn z O2 (x ≥ 0.8) is considered to be one of the ideal positive electrode materials in power batteries due to its high specific capacity, higher discharge voltage, low toxicity and low cost.

[0003] CN110416540A provides a high-nickel ternary positive electrode material and a preparation method thereof. The method comprises step 1, uniformly dispersing a high-nickel ternary metal salt and nanocellulose fibers in deionized water by ultrasonic dispersion and then standing to obtain a mixed system A; step 2, combining the mixed system A with a precipitant, and preparing a precursor of the high-nickel ternary positive electrode material by a hydrothermal method or a co-precipitation method; step 3, uniformly mixing the precursor of the high-nickel ternary positive electrode material with a lithium source, and calcining at 600-900° C. for 8-24 hours in an oxygen atmosphere to obtain the high-nickel ternary positive electrode material.

[0004] CN107910531A relates to a method for preparing a high nickel-based ternary positive electrode material, in particular to a method for preparing LiNi 0.85 Mn 0.1 Co 0.05 O2 ternary positive electrode material method. The method is characterized by the following steps: (1) preparing a ternary nickel, manganese, cobalt metal salt aqueous solution, a mixed alkali aqueous solution and a reaction base liquid; (2) adding the metal salt aqueous solution and the mixed alkali aqueous solution to the base liquid at a certain flow rate for microwave constant temperature reaction; (3) after the microwave reaction is completed, the reaction product is transferred to a hydrothermal reactor for hydrothermal treatment; (4) the coprecipitate after hydrothermal treatment is filtered, washed and dried; (5) the dried coprecipitate is mixed with lithium salt and ground, and then placed in a sintering furnace for high temperature solid phase reaction to obtain a method for preparing LiNi 0.85 Mn 0.1 Co 0.05 O2 ternary positive electrode material.

[0005] The high-nickel positive electrode material prepared in the above-mentioned literature mainly adopts the co-precipitation process for the nickel-cobalt-manganese ternary precursor. This process often requires a long synthesis time and has strict requirements on the parameter control of the reaction process, and the growth rate and morphology consistency of the particles are low. In addition, the obtained precursor needs to be washed to remove impurity elements, generating a large amount of waste water. At the same time, the obtained high-nickel positive electrode material still has defects such as mixed cations and residual alkali on the surface. The emergence of the above-mentioned problems makes the high-nickel positive electrode material still have capacity attenuation and poor thermal stability during the cycle process.

[0006] Therefore, how to improve the capacity decay and poor thermal stability of high-nickel positive electrode materials during the cycle process and simplify the preparation process is currently in urgent need of research. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a doped coated high nickel positive electrode material and its preparation method and application. The preparation method provided by the present invention realizes the uniform distribution of aluminum in the high nickel material through spray pyrolysis, avoids the occurrence of aluminum segregation, and cooperates with the coating of cerium dioxide to effectively improve the cycle performance, conductivity and thermal stability of the material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a doped coated high nickel cathode material, the preparation method comprising the following steps:

[0010] Spray pyrolysis of a nickel-cobalt-manganese-aluminum mixed salt solution to obtain a nickel-cobalt-manganese-aluminum precursor;

[0011] Mixing a nickel-cobalt-manganese-aluminum precursor, a lithium source and a cerium source, and sintering to obtain the doped and coated high-nickel positive electrode material;

[0012] Wherein, taking the total molar amount of nickel, cobalt and manganese as 100%, the molar proportion of nickel is ≥80%, for example, 80%, 83%, 85%, 88%, 90%, 93%, 95% or 98%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] The preparation method provided by the present invention reduces the segregation degree of metal ions through the spray pyrolysis method, and the obtained product has uniform components, thereby achieving the purpose of uniformly doping aluminum in the bulk phase of the high-nickel positive electrode material, and effectively reducing the degree of Li / Ni mixing, thereby improving the cycle stability and rate performance of the positive electrode material. In addition, during the sintering process, the oxide precursor obtained by spray pyrolysis can make lithium ions more easily and fully embedded in the oxide lattice structure, thereby improving the lattice stability of the material; at the same time, it cooperates with the subsequent one-step sintering of the cerium oxide coating to improve the transmission rate of lithium ions, avoid the contact between the internal material and the electrolyte, and reduce the interface side reaction; in addition, the preparation method provided by the present invention greatly reduces the mixing of impurities, reduces the difficulty of subsequent washing and filtering of the precursor material, greatly shortens the process flow, and at the same time reduces the generation of wastewater and reduces the production cost.

[0014] In the present invention, if aluminum is doped without spray pyrolysis, but a conventional co-precipitation method is used, aluminum segregation is likely to occur, especially when high aluminum content is doped, the segregation is more serious, and in order to precipitate uniformly, Al is often fed separately from the ternary liquid in the form of sodium aluminate solution; the present application simplifies the preparation process, and aluminum, especially high aluminum content doping, can be achieved without the addition of additional auxiliary substances such as dispersants or stabilizers; at the same time, if the subsequent cerium oxide coating treatment is not coordinated, the problem of electrolyte corrosion of the positive electrode material and the damage of the residual alkali on the surface of the material to the acidity and alkalinity of the battery cannot be solved; that is, in the present application, spray pyrolysis aluminum doping and cerium oxide coating must be coordinated to significantly improve the cycle stability and rate performance of the positive electrode material.

[0015] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] Preferably, based on the total molar amount of nickel, cobalt, manganese and aluminum as 100%, the molar amount of aluminum accounts for 1-5%, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] In the preparation method provided by the present invention, uniform doping of high aluminum content in high nickel positive electrode materials can be achieved.

[0018] Preferably, in the nickel-cobalt-manganese-aluminum mixed salt solution, the aluminum salt includes aluminum sulfate.

[0019] In the present invention, the aluminum salt does not need to be additionally selected as aluminate, and conventional aluminum sulfate can be used for the reaction, and there is no need to add auxiliary substances such as dispersants or stabilizers.

[0020] Preferably, the total concentration of metal ions in the nickel-cobalt-manganese-aluminum mixed salt solution is 1 to 2.5 mol / L, for example, 1 mol / L, 1.25 mol / L, 1.5 mol / L, 1.75 mol / L, 2 mol / L, 2.25 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the spray pyrolysis comprises:

[0022] A nickel-cobalt-manganese-aluminum mixed salt solution is atomized, and the atomized droplets are pyrolyzed to obtain a nickel-cobalt-manganese-aluminum precursor;

[0023] Preferably, the feed rate of the atomized droplets is 0.1 to 1 L / min, for example, 0.1 L / min, 0.2 L / min, 0.3 L / min, 0.4 L / min, 0.5 L / min, 0.6 L / min, 0.7 L / min, 0.8 L / min, 0.9 L / min or 1 L / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the pyrolysis method comprises flame pyrolysis.

[0025] In the present invention, the flame pyrolysis method is used for pyrolysis treatment, so that the atomized droplets can form uniform and fine precursor powder more quickly; and the fuel selected for the flame pyrolysis is a conventional technical solution, including methane and the like.

[0026] Preferably, the pyrolysis atmosphere comprises an oxygen-containing atmosphere.

[0027] In the present invention, the oxygen-containing atmosphere includes an oxygen atmosphere or an air atmosphere, etc.; carrying out the reaction in an oxygen-containing atmosphere is more conducive to the oxidation of the precursor.

[0028] Preferably, the pyrolysis temperature is 600-1200°C, for example 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the added amount of the cerium source is 0.2-1wt% of the mass of the nickel-cobalt-manganese-aluminum precursor, for example, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt%, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0030] In the present invention, the amount of cerium source added is adjusted to 0.2-1 wt%, which can better improve the transmission rate of lithium ions and increase the conductivity and stability of the material.

[0031] Preferably, the sintering temperature is 600-1000°C, for example 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the sintering time is 8 to 20 h, for example 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] As a preferred technical solution, the preparation method comprises the following steps:

[0034] A nickel-cobalt-manganese-aluminum mixed salt solution having a total metal ion concentration of 1 to 2.5 mol / L is atomized, and the atomized droplets are pyrolyzed at 600 to 1200° C. by flame pyrolysis at a feed rate of 0.1 to 1 L / min in an oxygen-containing atmosphere to obtain a nickel-cobalt-manganese-aluminum precursor;

[0035] Mixing a nickel-cobalt-manganese-aluminum precursor, a lithium source and a cerium source, wherein the amount of the cerium source added is 0.2-1wt% of the mass of the nickel-cobalt-manganese-aluminum precursor, and sintering at 600-1000° C. for 8-20 hours to obtain the doped and coated high-nickel positive electrode material;

[0036] Wherein, based on the total molar amount of nickel, cobalt and manganese as 100%, the molar proportion of nickel is ≥80%; based on the total molar amount of nickel, cobalt, manganese and aluminum as 100%, the molar proportion of aluminum is 1-5%.

[0037] It should also be noted that:

[0038] The lithium source provided by the present invention is selected by conventional technology, and the lithium source includes but is not limited to lithium hydroxide, lithium carbonate or lithium nitrate;

[0039] Optionally, the molar ratio of lithium in the lithium source to the sum of the molar amounts of metal elements in the nickel-cobalt-manganese-aluminum precursor is (1-1.05):1, for example, 1:1, 1.01:1, 1.02:1, 1.03:1, 1.04:1 or 1.05:1.

[0040] In a second aspect, the present invention provides a doped and coated high-nickel positive electrode material, wherein the doped and coated high-nickel positive electrode material is prepared by the preparation method described in the first aspect.

[0041] In a third aspect, the present invention further provides a lithium-ion battery, wherein the lithium-ion battery comprises the doped and coated high-nickel positive electrode material as described in the second aspect.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The preparation method provided by the present invention reduces the segregation degree of metal ions through the spray pyrolysis method, and the obtained product has uniform components, thereby achieving the purpose of uniformly doping aluminum in the bulk phase of the high-nickel positive electrode material, and effectively reducing the degree of Li / Ni mixing, thereby improving the cycle stability and rate performance of the positive electrode material. In addition, during the sintering process, the oxide precursor obtained by spray pyrolysis can make lithium ions more easily and fully embedded in the oxide lattice structure, thereby improving the lattice stability of the material; at the same time, it cooperates with the subsequent one-step sintering of the cerium oxide coating to improve the transmission rate of lithium ions, avoid the contact between the internal material and the electrolyte, and reduce the interface side reaction; in addition, the preparation method provided by the present invention greatly reduces the mixing of impurities, reduces the difficulty of subsequent washing and filtering of the precursor material, greatly shortens the process flow, and at the same time reduces the generation of wastewater and reduces the production cost. DETAILED DESCRIPTION

[0044] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0046] Example 1

[0047] This embodiment provides a method for preparing a doped coated high nickel positive electrode material, the preparation method is as follows:

[0048] (1) nickel sulfate, cobalt sulfate and manganese sulfate solutions are mixed in a certain ratio (nickel:cobalt:manganese=8:1:1) with a metal ion concentration of 2 mol / L; then aluminum sulfate crystals are added to the solution so that the molar ratio of aluminum to nickel, cobalt and manganese is 1:99, and the mixture is stirred thoroughly to obtain a mixed solution of nickel, cobalt, manganese and aluminum;

[0049] (2) atomizing the mixed solution prepared in step (1) in an atomization zone; using methane as a fuel in a flame synthesis zone under an air atmosphere; spraying nitrogen as a carrier gas carrying atomized droplets into the flame synthesis zone at a rate of 0.2 L / min for spray pyrolysis at a pyrolysis temperature of 800° C. to obtain a nickel-cobalt-manganese-aluminum oxide precursor;

[0050] (3) The nickel-cobalt-manganese-aluminum oxide precursor, lithium hydroxide and cerium dioxide of step (2) are mixed thoroughly, wherein the molar ratio of lithium to nickel-cobalt-manganese-aluminum is 1.05:1, and the cerium content is 0.2% (the amount of cerium dioxide added is 0.2% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor), and then sintered at 700°C for 10 hours to obtain a cerium dioxide-coated nickel-cobalt-manganese-aluminum positive electrode material.

[0051] Example 2

[0052] This embodiment provides a method for preparing a doped coated high nickel positive electrode material, the preparation method is as follows:

[0053] (1) nickel sulfate, cobalt sulfate and manganese sulfate solutions are mixed in a certain ratio (nickel:cobalt:manganese=8:1:1) with a metal ion concentration of 2 mol / L; then aluminum sulfate crystals are added to the solution so that the molar ratio of aluminum to nickel, cobalt and manganese is 2:98, and the mixture is stirred thoroughly to obtain a mixed solution of nickel, cobalt, manganese and aluminum;

[0054] (2) atomizing the mixed solution prepared in step (1) in an atomization zone; using methane as a fuel in a flame synthesis zone under an air atmosphere; spraying nitrogen as a carrier gas carrying atomized droplets into the flame synthesis zone at a rate of 0.2 L / min for spray pyrolysis at a pyrolysis temperature of 800° C. to obtain a nickel-cobalt-manganese-aluminum oxide precursor;

[0055] (3) The nickel-cobalt-manganese-aluminum oxide precursor, lithium hydroxide and cerium dioxide of step (2) are mixed thoroughly, wherein the molar ratio of lithium to nickel-cobalt-manganese-aluminum is 1.05:1 and the cerium content is 0.2% (the amount of cerium dioxide added is 0.2% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor), and then sintered at 600° C. for 14 h to obtain a cerium dioxide-coated nickel-cobalt-manganese-aluminum positive electrode material.

[0056] Example 3

[0057] This embodiment provides a method for preparing a doped coated high nickel positive electrode material, the preparation method is as follows:

[0058] (1) mixing nickel sulfate, cobalt sulfate and manganese sulfate solutions in a certain ratio (nickel:cobalt:manganese=8:1:1) with a metal ion concentration of 1.5 mol / L; then adding aluminum sulfate crystals to the solution so that the molar ratio of aluminum to nickel, cobalt and manganese is 5:95, and stirring thoroughly to obtain a mixed solution of nickel, cobalt, manganese and aluminum;

[0059] (2) atomizing the mixed solution prepared in step (1) in an atomization zone; using methane as a fuel in a flame synthesis zone under an air atmosphere; spraying nitrogen as a carrier gas carrying atomized droplets into the flame synthesis zone at a rate of 1 L / min for spray pyrolysis at a pyrolysis temperature of 1000° C. to obtain a nickel-cobalt-manganese-aluminum oxide precursor;

[0060] (3) The nickel-cobalt-manganese-aluminum oxide precursor, lithium hydroxide and cerium dioxide of step (2) are mixed thoroughly, wherein the molar ratio of lithium to nickel-cobalt-manganese-aluminum is 1.05:1, and the cerium content is 0.2% (the amount of cerium dioxide added is 0.2% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor), and then sintered at 700°C for 10 hours to obtain a cerium dioxide-coated nickel-cobalt-manganese-aluminum positive electrode material.

[0061] Example 4

[0062] The difference between this embodiment and embodiment 1 is that the amount of cerium dioxide added in step (3) of this embodiment is 0.5% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor.

[0063] The rest of the preparation methods and parameters were the same as those in Example 1.

[0064] Example 5

[0065] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of cerium dioxide added is 1% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor.

[0066] The rest of the preparation methods and parameters were the same as those in Example 1.

[0067] Example 6

[0068] The difference between this embodiment and embodiment 1 is that in step (2) of this embodiment, a non-flame pyrolysis method is adopted. Instead, a nitrogen carrier gas is used to spray the atomized droplets into a reactor (pyrolysis furnace) heated by a spray pyrolysis device, and the pyrolysis pressure is 0.25 MPa.

[0069] The rest of the preparation methods and parameters were the same as those in Example 1.

[0070] Example 7

[0071] The difference between this embodiment and embodiment 1 is that the atmosphere for spray pyrolysis in step (2) of this embodiment is not an oxygen atmosphere but a pure nitrogen atmosphere.

[0072] The rest of the preparation methods and parameters were the same as those in Example 1.

[0073] Example 8

[0074] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of cerium dioxide added is 1.5% of the mass of the nickel-cobalt-manganese-aluminum oxide precursor.

[0075] The rest of the preparation methods and parameters were the same as those in Example 1.

[0076] Comparative Example 1

[0077] The difference between this comparative example and Example 1 is that step (1) of this comparative example does not contain aluminum salt, that is, no aluminum doping is performed.

[0078] The rest of the preparation methods and parameters were the same as those in Example 1.

[0079] Comparative Example 2

[0080] The difference between this comparative example and Example 1 is that the method for preparing the nickel-cobalt-manganese-aluminum precursor in this comparative example is a coprecipitation method, which is as follows:

[0081] Mix nickel sulfate, cobalt sulfate and manganese sulfate solutions in a certain ratio (nickel:cobalt:manganese=8:1:1) with a metal ion concentration of 2 mol / L; then add aluminum sulfate crystals to the solution so that the molar ratio of aluminum to nickel, cobalt and manganese is 1:99, and stir thoroughly to obtain a mixed solution of nickel, cobalt, manganese and aluminum;

[0082] The prepared mixed solution, precipitant solution (sodium hydroxide solution) and complexing agent solution (ammonia solution) are added to the reactor in parallel, with flow rates of 40 L / h, 12 L / h and 8 L / h respectively; during the reaction, the flow rate is adjusted to keep the pH between 11-12, the ammonia concentration is 6-8 g / L, and the reaction temperature is maintained at 50°C; when D50 reaches the target particle size (4 μm), the feeding is stopped, and washing and drying are performed to obtain a nickel-cobalt-manganese-aluminum precursor;

[0083] The sintering process of step (3) is consistent with that of Example 1.

[0084] Comparative Example 3

[0085] The difference between this comparative example and Example 1 is that cerium dioxide is not added in step (3) of this comparative example.

[0086] The rest of the preparation methods and parameters were the same as those in Example 1.

[0087] [Preparation and performance testing of lithium-ion batteries]

[0088] The high nickel positive electrode materials provided in Examples 1-8 and Comparative Examples 1-3 were respectively used to prepare lithium ion batteries, and the specific preparation process was as follows:

[0089] The positive electrode material, conductive carbon black SP (TIMCAL), and polyvinylidene fluoride PVDF (HSV900) are mixed in a mass ratio of 90:5:5, and the solvent is N-methylpyrrolidone. The slurry is evenly coated on the aluminum foil with a scraper with a coating gap of 100μm. After coating, it is first dried at 120℃ with air blast, then rolled, and finally the dried electrode is cut into Φ12 circular electrode sheets. After vacuum drying at 120℃, the electrode sheet is weighed to obtain the positive electrode sheet of the button half-cell; the negative electrode uses a Φ14 metal lithium sheet, the separator is a Φ19 PP microporous membrane (Celgard2400), and the electrolyte uses a lithium battery basic electrolyte, that is, EC and DEC are used as a mixed solvent in a volume ratio of 1:1, and 1.1mol / L LiPF6 is added. The positive electrode sheet, metal lithium sheet, separator and electrolyte are assembled to obtain a button battery.

[0090] The lithium ion batteries provided in Examples 1-8 and Comparative Examples 1-3 were respectively subjected to performance tests. The test conditions were: the electrochemical properties of the positive electrode materials were tested at a rate of 0.1C within a voltage range of 2.8-4.3V. The test results are shown in Table 1.

[0091] Table 1

[0092]

[0093] From Table 1, we can get:

[0094] From the data results of Examples 1-5, it can be seen that the present invention selects a specific spray pyrolysis method to carry out bulk doping of aluminum in high-nickel positive electrode materials, and cooperates with cerium oxide coating to effectively reduce the degree of Li / Ni mixing in high-nickel positive electrode materials; improves structural stability, avoids contact between internal materials and electrolyte, and reduces interfacial side reactions; thereby improving the cycle stability and capacity of the material.

[0095] It can be seen from the data results of Example 1 and Example 6 that the use of a non-flame pyrolysis method is not conducive to improving the uniformity of the precursor morphology, thereby reducing the charge and discharge capacity and cycle stability of the positive electrode material.

[0096] It can be seen from the data results of Example 1 and Example 7 that if the pyrolysis process is not carried out in an oxygen-containing atmosphere, pre-oxidation of the precursor cannot be achieved, and the subsequent sintering process may prevent lithium ions from being fully embedded in the lattice structure, which is not conducive to improving the structural stability of the material.

[0097] It can be seen from the data results of Example 1 and Example 8 that if the coating amount of cerium oxide is too much, the interface mass transfer impedance will increase and the conductive properties of the material will be affected.

[0098] It can be seen from the data results of Example 1 and Comparative Examples 1-3 that the aluminum doping by spray pyrolysis and the cerium oxide coating must be coordinated and neither is indispensable. The lack of any one of the conditions will lead to a decrease in the material capacity and cycle stability.

[0099] In summary, the preparation method provided by the present invention reduces the degree of segregation of metal ions through spray pyrolysis, and the obtained product has uniform components, thereby achieving the purpose of uniformly doping aluminum in the bulk phase of the high-nickel positive electrode material, and effectively reducing the degree of Li / Ni mixing, thereby improving the cycle stability and rate performance of the positive electrode material. In addition, the oxide precursor obtained by spray pyrolysis can make lithium ions more easily and fully embedded in the oxide lattice structure during the sintering process, thereby improving the lattice stability of the material; at the same time, it cooperates with the subsequent one-step sintering of the cerium oxide coating to improve the transmission rate of lithium ions, avoid the contact between the internal material and the electrolyte, and reduce the interface side reactions; in addition, the preparation method provided by the present invention greatly reduces the mixing of impurities, reduces the difficulty of subsequent washing and filtering of the precursor material, greatly shortens the process flow, and at the same time reduces the generation of wastewater and reduces production costs.

[0100] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a doped and coated high-nickel positive electrode material, characterized in that: The preparation method comprises the following steps: Spray pyrolysis of a nickel-cobalt-manganese-aluminum mixed salt solution to obtain a nickel-cobalt-manganese-aluminum precursor; Mixing a nickel-cobalt-manganese-aluminum precursor, a lithium source and a cerium source, and sintering to obtain the doped and coated high-nickel positive electrode material; Wherein, based on the total molar amount of nickel, cobalt and manganese as 100%, the molar proportion of nickel is ≥80%.

2. The method for preparing a doped and coated high-nickel positive electrode material according to claim 1, characterized in that: Based on the total molar amount of nickel, cobalt, manganese and aluminum being 100%, the molar amount of aluminum accounts for 1 to 5%.

3. The method for preparing a doped and coated high-nickel positive electrode material according to claim 1 or 2, characterized in that: In the nickel-cobalt-manganese-aluminum mixed salt solution, the aluminum salt includes aluminum sulfate; Preferably, the total concentration of metal ions in the nickel-cobalt-manganese-aluminum mixed salt solution is 1 to 2.5 mol / L.

4. The method for preparing a doped and coated high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The spray pyrolysis comprises: The nickel-cobalt-manganese-aluminum mixed salt solution is atomized, and the atomized droplets are pyrolyzed to obtain a nickel-cobalt-manganese-aluminum precursor.

5. The method for preparing a heterogeneous coated high nickel positive electrode material according to claim 4, characterized in that: The feed rate of the atomized droplets is 0.1 to 1 L / min; Preferably, the pyrolysis method comprises flame pyrolysis; Preferably, the pyrolysis atmosphere comprises an oxygen-containing atmosphere; Preferably, the pyrolysis temperature is 600-1200°C.

6. The method for preparing a doped and coated high-nickel positive electrode material according to any one of claims 1 to 5, characterized in that: The amount of the cerium source added is 0.2-1 wt % of the mass of the nickel-cobalt-manganese-aluminum precursor.

7. The method for preparing a doped and coated high-nickel positive electrode material according to any one of claims 1 to 6, characterized in that: The sintering temperature is 600-1000° C., and the sintering time is 8-20 hours.

8. The method for preparing a doped and coated high-nickel positive electrode material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: A nickel-cobalt-manganese-aluminum mixed salt solution having a total metal ion concentration of 1 to 2.5 mol / L is atomized, and the atomized droplets are pyrolyzed at 600 to 1200° C. by flame pyrolysis at a feed rate of 0.1 to 1 L / min in an oxygen-containing atmosphere to obtain a nickel-cobalt-manganese-aluminum precursor; Mixing a nickel-cobalt-manganese-aluminum precursor, a lithium source and a cerium source, wherein the amount of the cerium source added is 0.2-1wt% of the mass of the nickel-cobalt-manganese-aluminum precursor, and sintering at 600-1000° C. for 8-20 hours to obtain the doped and coated high-nickel positive electrode material; Wherein, based on the total molar amount of nickel, cobalt and manganese as 100%, the molar proportion of nickel is ≥80%; based on the total molar amount of nickel, cobalt, manganese and aluminum as 100%, the molar proportion of aluminum is 1-5%.

9. A doped and coated high nickel positive electrode material, characterized in that: The doped and coated high-nickel positive electrode material is prepared by the preparation method according to any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the doped and coated high-nickel positive electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Method for preparing positive electrode material for lithium ion cell by spraying, combusting and pyrolyzing

    CN105932269A

  • Modified lithium nickel cobalt manganese oxide ternary positive electrode material and preparation method and application thereof

    CN111320214A

  • Cation co-doped lithium-rich manganese-based material as well as preparation method and application thereof

    CN118231639A

  • Submicron small-particle-size lithium-rich manganese-based precursor as well as preparation method and application thereof

    CN118255402A

  • High-dispersion high-nickel single-crystal lithium nickel cobalt manganate positive electrode material and preparation method thereof

    CN118270857A