Method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method and application of ferrous sulfide-based autotrophic denitrification filler

The sulfhydryl-based autotrophic denitrification filler prepared by mechanochemical method solves the problem of low bioavailability of the elemental sulfur-driven autotrophic denitrification system, achieves efficient nitrogen removal and phosphorus removal effect and process stability, and reduces sulfate Generate, suitable for use in sewage treatment and other applications.

CN118878074AActive Publication Date: 2024-11-01CHANGJIANG RIVER SCI RES INST CHANGJIANG WATER RESOURCES COMMISSION

Patent Information

Application Number
CN202411062516.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing autotrophic denitrification system driven by elemental sulfur has low bioavailability, resulting in insufficient denitrification efficiency, process safety and stability, and high sulfate concentration, which limits its application.

Method used

Mechanical chemistry method is used to prepare sulfide-based autotrophic denitrification fillers, and ball milling of elemental sulfur, divalent iron source and activated carbon powder to form a molten composite material, which is cooled and broken to form a sulfide-based iron with various sulfur forms and semiconductor characteristics. Fillers to improve bioavailability and nitrogen removal and phosphorus removal effect.

Benefits of technology

It significantly improves the bioavailability and nitrogen removal effect of sulfide-based autotrophic denitrification fillers, and is safe in process and low in cost, and is easy to produce on a large scale. The filler body phase is uniform and the size is controllable, which reduces the production of sulfate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878074A_ABST
    Figure CN118878074A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a sulfur-iron-based autotrophic denitrification filler by a mechanochemical method and application of the sulfur-iron-based autotrophic denitrification filler, and the method comprises the following steps: putting elemental sulfur powder, a ferrous iron source and activated carbon powder into a ball mill for ball milling for 2-4 hours to obtain a powdery composite material; heating and melting the powdery composite material to obtain a molten composite material; the molten composite material is granulated and then cooled, or the molten composite material is directly cooled and solidified and then crushed, and the ferrous sulfide-based autotrophic denitrification filler is obtained; the total mass percent of the elemental sulfur powder and the ferrous iron source is 80%-90%, and the mass percent of the activated carbon powder is 10%-20%; the mass ratio of the elemental sulfur powder to the ferrous iron source is (1: 1)-(7: 3). The nitrogen and phosphorus removal effect of the prepared sulfur-iron-based autotrophic denitrification filler is enhanced, and the sulfur-iron-based autotrophic denitrification filler can be applied to nitrogen and phosphorus removal of effluent of a secondary sedimentation tank of a sewage treatment plant, constructed wetlands, industrial wastewater and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of deep denitrification and phosphorus removal, and specifically relates to a method for preparing sulfide-iron-based autotrophic denitrification filler by a mechanochemical method and its application. Background Art

[0002] Elemental sulfur S 0 Driven autotrophic denitrification is regarded as the process with the greatest prospects for large-scale application. Compared with heterotrophic denitrification systems, elemental sulfur-driven autotrophic denitrification has the advantages of more thorough denitrification, low cost and low risk, but the existing system still has the risks of low bioavailability, low effluent pH and high sulfate concentration, which restricts the denitrification efficiency, process safety and process stability of autotrophic denitrification. Therefore, there is an urgent need for autotrophic denitrification fillers with high denitrification efficiency, good stability, and green safety. The key issue limiting the performance and application of elemental sulfur-driven autotrophic denitrification is the low bioavailability of elemental sulfur. Low water solubility, strong hydrophobicity and poor biocompatibility are the main reasons for the low bioavailability of elemental sulfur. In addition, elemental sulfur is soft and light, and is easily retained with the effluent, which also reduces the utilization rate.

[0003] The combination of sulfur and iron-containing minerals can improve denitrification performance, alleviate pH reduction and sulfate production, and the introduction of iron-containing minerals can achieve simultaneous phosphorus removal on the basis of nitrogen removal. At present, most methods of combining sulfur and iron-containing minerals to prepare sulfur-iron-based autotrophic denitrification fillers are: mixing sulfur and iron-containing minerals and then melting and granulating, or melting sulfur and then adding iron-containing minerals to mix and granulate. However, there is still room for further improvement in the bioavailability and nitrogen and phosphorus removal effects of sulfur-iron-based autotrophic denitrification fillers. Summary of the invention

[0004] The purpose of the present application is to provide a method and application for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method, wherein the bioavailability of the prepared ferrous sulfide-based autotrophic denitrification filler is improved, and deep nitrogen and phosphorus removal is enhanced.

[0005] On the one hand, the present application provides a method for preparing a sulfide-iron-based autotrophic denitrification filler by a mechanochemical method, comprising:

[0006] Taking elemental sulfur powder, a divalent iron source and activated carbon powder, placing them in a ball mill for 2 to 4 hours to obtain a powdered composite material;

[0007] heating and melting the powdered composite material to obtain a molten composite material;

[0008] The molten composite material is first granulated and then cooled, or the molten composite material is directly cooled and solidified and then crushed to obtain the sulfide-iron-based autotrophic denitrification filler;

[0009] The total mass percentage of the elemental sulfur powder and the divalent iron source is 80% to 90%, the mass percentage of the activated carbon powder is 10% to 20%; and the mass ratio of the elemental sulfur powder to the divalent iron source is 1:1 to 7:3.

[0010] Furthermore, the mass ratio of elemental sulfur powder to divalent iron source is preferably 7:3.

[0011] In some embodiments, the ferrous iron source is selected from ferrous carbonate and / or ferrous sulfide, preferably ferrous sulfide.

[0012] In some embodiments, the powdered composite material is heated and melted, specifically: the powdered composite material is heated to 120° C. to 140° C. to melt it.

[0013] In some embodiments, the rotation speed of the ball mill is 200-600 rpm, preferably 400 rpm.

[0014] In some embodiments, the mass ratio of the ball milling medium to the raw material is 4:1, and the raw material includes elemental sulfur powder, a divalent iron source, and activated carbon powder; the ball milling medium can be selected from stainless steel ball milling beads.

[0015] The method of the present application uses solid matter as raw material, and utilizes a mechanochemical method based on high-energy ball milling to pretreat the raw material to assist in the preparation of sulfide-iron-based autotrophic denitrification filler. The prepared sulfide-iron-based autotrophic denitrification filler has a uniform phase and controllable size, and the nitrogen and phosphorus removal effects are significantly improved.

[0016] During the ball milling process, the ball milling medium collides with the solid raw material at high speed, thereby introducing a large number of defects into the solid particles, forming a metastable state and increasing the surface activity of the particles. In the metastable state, elemental sulfur powder can form a variety of different sulfur forms, and elemental sulfur powder can generate solid sulfur ions S in situ. n 2- On the one hand, sulfur ion S n 2- It can reduce the hydrophobicity of elemental sulfur powder, which helps to improve the bioavailability of elemental sulfur powder. On the other hand, sulfur ion S n 2- Can promote microorganisms and S 0 The electron transfer between particles helps to enhance the effect and efficiency of nitrogen removal and phosphorus removal. The preferred source of divalent iron is ferrous sulfide, which can generate FeS with semiconductor properties in situ during the ball milling process. n , which can further promote electron transfer and help achieve better nitrogen and phosphorus removal effects and efficiency.

[0017] On the other hand, the present application provides the use of the sulfide-iron-based autotrophic denitrification filler prepared by the above method in the denitrification and phosphorus removal process, for example, it can be applied to the denitrification and phosphorus removal of the effluent from the secondary sedimentation tank of a sewage treatment plant, artificial wetlands, and industrial wastewater.

[0018] In some embodiments, the dosage of the sulfide-iron-based autotrophic denitrification filler is 20-40 g / L.

[0019] Compared with the prior art, this application has the following advantages and beneficial effects:

[0020] (1) The method of the present application has safe raw materials, stable ingredients, and low cost; the preparation process does not use solvents, is green, environmentally friendly, efficient, and easy to scale up for production.

[0021] (2) This application introduces high-energy ball milling to pre-treat the solid raw materials. The elemental sulfur powder can generate various sulfur forms in situ, which increases the content of polysulfide in the filler and avoids the shortcomings of the elemental sulfur powder itself (low water solubility, strong hydrophobicity, etc.); and high-energy ball milling also introduces a large number of defects to the solid particles, which can significantly improve the surface activity of the particles. Compared with the traditional method, the filler prepared by the method of this application has a uniform phase, controllable size, and the denitrification and phosphorus removal effect is also significantly enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is the XPS spectrum of the sample in Example 1;

[0023] Figure 2 The form and proportion of sulfur in the sample of Example 1;

[0024] Figure 3 It is a comparison chart of the denitrification rates of samples of the embodiment and the comparative example;

[0025] Figure 4 It is the phosphorus removal efficiency of the samples of the embodiments and comparative examples. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and beneficial effects of the present application more clear, the present application is further described in detail below in conjunction with embodiments.

[0027] Example 1

[0028] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0029] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0030] (2) 56 g of elemental sulfur powder, 24 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0031] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0032] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0033] Figure 1 The XPS spectrum of the sample in this example is shown. From the XPS spectrum, it can be seen that the sample contains S n 2- . Figure 2 The sulfur forms and the proportions of each sulfur form in the samples of this embodiment are shown. Figure 2 It can be seen that the sulfur element in the samples of this embodiment is not only in the form of single substance S 0 The form exists, including S n 2- 、S2 2- 、SO4 2- 、SO3 2- Sulfur forms, especially S n 2- , which is an extracellular redox mediator that promotes the 0 The transfer of electrons between particles is beneficial to promoting significant improvements in the nitrogen and phosphorus removal effects.

[0034] The following method was used to test the dephosphorization and nitrogen removal effects of the samples in this embodiment, including:

[0035] (1) Synthetic sewage was prepared according to the concentration of the main pollutants in the secondary effluent: KNO3, KH2PO4, NaHCO3, MgCl2·6H2O and FeSO4·7H2O were added to deionized water; the concentration of KNO3 was 0.3 g / L, the concentration of nitrate nitrogen NO3-N was 20 mg / L, the concentration of KH2PO4 was 0.0509 g / L, the total phosphorus concentration was 10 mg / L, the concentration of NaHCO3 was 0.1 g / L, the concentration of MgCl2·6H2O was 0.1 g / L, and the concentration of FeSO4·7H2O was 0.005 g / L.

[0036] (2) Take 1000 mL of synthetic sewage and add it to a 1000 mL conical flask, add 30 g of sulfide-based autotrophic denitrification filler sample, then add activated sludge suspension, and finally cover the conical flask with a rubber stopper and seal it. Punch a hole in the rubber stopper and insert it into a glass tube with a diameter of 0.8 cm. At the same time, the glass tube is connected to a rubber tube and the rubber stopper is fastened.

[0037] (3) Nitrogen was introduced into the conical flask through the rubber tube for 15 min, and the rubber tube was sealed with a water stop clamp. The conical flask was then placed in a constant temperature shaker, the temperature was set to 30°C, the speed was set to 150 rpm, and sampling was performed at a fixed time. When sampling, 5 mL was extracted using a disposable syringe, and the nitrate nitrogen and total phosphorus contents of the sample were quickly determined after passing through a 0.45 μm filter membrane, and the nitrogen removal rate and total phosphorus removal rate were calculated.

[0038] According to the test, the nitrogen removal rates of the sample in this embodiment were 11.1%, 27.8% and 100% respectively when the reaction time was 30min, 2h and 98h, and the total phosphorus removal rate could reach 87.3%.

[0039] Example 2

[0040] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0041] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0042] (2) 40 g of elemental sulfur powder, 40 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0043] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0044] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0045] The dephosphorization and nitrogen removal effects of the samples of this embodiment were tested using the same method as in Example 1. After testing, the nitrogen removal rates of the samples of this embodiment were 10.1%, 11.2% and 77.0% respectively when the reaction time was 30 min, 2 h and 98 h, and the total phosphorus removal rate was as high as 95.8%.

[0046] Example 3

[0047] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0048] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0049] (2) 24 g of elemental sulfur powder, 56 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0050] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0051] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0052] The dephosphorization and denitrification effects of the samples of this embodiment were tested in the same manner as in Example 1. After testing, the nitrogen removal rates of the samples of this embodiment were 6.8% and 93.4% respectively after 30 minutes and 98 hours of reaction. However, in this embodiment, since the mass proportion of sulfur powder was too low, it was difficult to heat and melt, and granulation was difficult.

[0053] Example 4

[0054] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0055] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0056] (2) 56 g of elemental sulfur powder, 24 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 200 rpm, and the ball milling time was set to 4 h.

[0057] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0058] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0059] The dephosphorization and nitrogen removal effects of the samples of this embodiment were tested using the same method as in Example 1. The test showed that the nitrogen removal rates of the samples of this embodiment were 14.7%, 17.7% and 63.8% when the reaction time was 30 min, 2 h and 98 h, respectively.

[0060] Example 5

[0061] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0062] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0063] (2) 56 g of elemental sulfur powder, 24 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 600 rpm, and the ball milling time was set to 4 h.

[0064] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0065] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0066] The dephosphorization and denitrification effect of the sample of this embodiment was tested in the same manner as in Example 1. After testing, the nitrogen removal rates of the sample of this embodiment were 10.8% and 99.8% at 30 minutes and 98 hours of reaction, respectively. However, in this embodiment, due to the excessively high ball milling energy, the material was easily agglomerated, and the sample yield was only about 30%. It should be noted that the yield refers to the mass ratio of the powdered filler obtained after the final screening to the mass of all raw materials.

[0067] Example 6

[0068] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0069] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0070] (2) 63 g of elemental sulfur powder, 27 g of ferrous carbonate and 10 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0071] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0072] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0073] The dephosphorization and denitrification effects of the samples in this embodiment were tested in the same manner as in Example 1. After testing, the nitrogen removal rates of the samples in this embodiment were 14.5% and 100% at 30 minutes and 98 hours of reaction, respectively. However, in this embodiment, the amount of activated carbon powder used was relatively low, accounting for only 10% of the total amount of materials used, the dispersibility was reduced, the materials were very easy to agglomerate, and the sample yield was low, about 70%.

[0074] Example 7

[0075] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0076] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0077] (2) 56 g of elemental sulfur powder, 24 g of ferrous sulfide and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0078] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0079] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0080] The dephosphorization and nitrogen removal effects of the samples of this embodiment were tested using the same method as in Example 1. After testing, the nitrogen removal rates of the samples of this embodiment were 3.2%, 4.8% and 96.3% respectively when the reaction time was 30 min, 2 h and 98 h, and the total phosphorus removal rate could reach 100%.

[0081] Example 8

[0082] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0083] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0084] (2) 56 g of elemental sulfur powder, 24 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0085] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0086] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0087] The following method was used to test the dephosphorization and nitrogen removal effects of the samples in this embodiment, including:

[0088] (1) Synthetic sewage was prepared according to the concentration of the main pollutants in the secondary effluent: KNO3, KH2PO4, NaHCO3, MgCl2·6H2O and FeSO4·7H2O were added to deionized water; the concentration of KNO3 was 0.6 g / L, the concentration of nitrate nitrogen NO3-N was 40 mg / L, the concentration of KH2PO4 was 0.0509 g / L, the total phosphorus concentration was 10 mg / L, the concentration of NaHCO3 was 0.1 g / L, the concentration of MgCl2·6H2O was 0.1 g / L, and the concentration of FeSO4·7H2O was 0.005 g / L.

[0089] (2) Take 1000 mL of synthetic sewage and add it to a 1000 mL conical flask, add 30 g of sulfide-based autotrophic denitrification filler sample, then add activated sludge suspension, and finally cover the conical flask with a rubber stopper and seal it. Punch a hole in the rubber stopper and insert it into a glass tube with a diameter of 0.8 cm. At the same time, the glass tube is connected to a rubber tube and the rubber stopper is fastened.

[0090] (3) Nitrogen was introduced into the conical flask through the rubber tube for 15 min, and the rubber tube was sealed with a water stop clamp. The conical flask was then placed in a constant temperature shaker, the temperature was set to 30°C, the speed was set to 150 rpm, and sampling was performed at a fixed time. When sampling, 5 mL was extracted using a disposable syringe, and the nitrate nitrogen and total phosphorus contents of the sample were quickly determined after passing through a 0.45 μm filter membrane, and the nitrogen removal rate and total phosphorus removal rate were calculated.

[0091] According to the test, the nitrogen removal rates of the sample in this embodiment were 10.2%, 10.9% and 19.3% respectively when the reaction time was 30min, 2h and 98h, and the total phosphorus removal rate could reach 87.3%.

[0092] Example 9

[0093] The specific steps of preparing the ferrous sulfide-based autotrophic denitrification filler in this embodiment are as follows:

[0094] (1) Place 400 g of stainless steel ball mill beads into a 500 mL stainless steel ball mill;

[0095] (2) 56 g of elemental sulfur powder, 24 g of ferrous carbonate and 20 g of activated carbon powder were placed in a stainless steel ball mill for ball milling. No atmosphere protection was required during the ball milling process, and room temperature and pressure were maintained. The speed of the planetary ball mill was set to 400 rpm, and the ball milling time was set to 4 h.

[0096] (3) After the ball milling is completed, the powdered composite material is taken out and the powdered composite material is heated to 140° C. to obtain a molten composite material;

[0097] (4) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0098] The following method was used to test the dephosphorization and nitrogen removal effects of the samples in this embodiment, including:

[0099] (1) Synthetic sewage was prepared according to the concentration of the main pollutants in the secondary effluent: KNO3, KH2PO4, NaHCO3, MgCl2·6H2O and FeSO4·7H2O were added to deionized water; the concentration of KNO3 was 0.15 g / L, the concentration of nitrate nitrogen NO3-N was 10 mg / L, the concentration of KH2PO4 was 0.0509 g / L, the total phosphorus concentration was 10 mg / L, the concentration of NaHCO3 was 0.1 g / L, the concentration of MgCl2·6H2O was 0.1 g / L, and the concentration of FeSO4·7H2O was 0.005 g / L.

[0100] (2) Take 1000 mL of synthetic sewage and add it to a 1000 mL conical flask, add 30 g of sulfide-based autotrophic denitrification filler sample, then add activated sludge suspension, and finally cover the conical flask with a rubber stopper and seal it. Punch a hole in the rubber stopper and insert it into a glass tube with a diameter of 0.8 cm. At the same time, the glass tube is connected to a rubber tube and the rubber stopper is fastened.

[0101] (3) Nitrogen was introduced into the conical flask through the rubber tube for 15 min, and the rubber tube was sealed with a water stop clamp. The conical flask was then placed in a constant temperature shaker, the temperature was set to 30°C, the speed was set to 150 rpm, and sampling was performed at a fixed time. When sampling, 5 mL was extracted using a disposable syringe, and the nitrate nitrogen and total phosphorus contents of the sample were quickly determined after passing through a 0.45 μm filter membrane, and the nitrogen removal rate and total phosphorus removal rate were calculated.

[0102] According to the test, the nitrogen removal rates of the sample in this embodiment were 6.2%, 8.3% and 100% respectively when the reaction time was 30min, 2h and 98h, and the total phosphorus removal rate could reach 87.3%.

[0103] It should be noted that, except for Examples 5 and 6, the sample yields of other Examples are all as high as over 95%.

[0104] Comparative Example 1

[0105] In this comparative example, the raw materials were not subjected to mechanochemical pretreatment when preparing the ferrous sulfide-based autotrophic denitrification filler. The specific steps are as follows:

[0106] (1) Take 56 g of elemental sulfur powder and heat it to 140° C. to melt the elemental sulfur powder;

[0107] (2) adding 24 g of ferrous carbonate and 20 g of activated carbon powder and stirring evenly to obtain a molten composite material;

[0108] (3) The molten composite material is directly cooled and solidified, and the obtained solid material is crushed to obtain a sulfide-iron-based autotrophic denitrification filler sample.

[0109] The dephosphorization and nitrogen removal effects of the comparative example samples were tested using the same method as in Example 1. After testing, the nitrogen removal rates of the samples in this example were 5.1%, 11.6% and 92.4% respectively when the reaction time was 30 min, 2 h and 98 h, and the total phosphorus removal rate reached 69.3%.

[0110] Comparative Example 2

[0111] In order to fully illustrate the advantages of the ferrous sulfur-based autotrophic denitrification filler prepared in the present application, this comparative example uses commercial sulfur particles as denitrification fillers to detect the dephosphorization and nitrogen removal effects, and the method is the same as the dephosphorization and nitrogen removal effect detection method in Example 1. After testing, the nitrogen removal rates of the comparative example samples were 6.3%, 8.1% and 23.4% respectively when the reaction time was 30min, 2h and 98h, and there was no dephosphorization effect.

[0112] Comparative Example 3

[0113] In order to fully illustrate the advantages of the sulfide iron-based autotrophic denitrification filler prepared in the present application, this comparative example uses commercial sulfide iron-based autotrophic denitrification materials as denitrification fillers, and performs dephosphorization and nitrogen removal effect detection on them, and the method is the same as the dephosphorization and nitrogen removal effect detection method in Example 1. After detection, the nitrogen removal rates of the samples in this comparative example were 7.0%, 10.5% and 93.4% respectively when the reaction time was 30min, 2h and 98h, and there was no dephosphorization effect.

[0114] Comparative Example 4

[0115] In order to eliminate the influence of chemical reduction of fillers on the experimental results, a control experiment without adding domesticated sludge was set up, including:

[0116] (1) Synthetic sewage was prepared according to the concentration of the main pollutants in the secondary effluent: KNO3, KH2PO4, NaHCO3, MgCl2·6H2O and FeSO4·7H2O were added to deionized water; the concentration of KNO3 was 0.3 g / L, the concentration of nitrate nitrogen NO3-N was 20 mg / L, the concentration of KH2PO4 was 0.0509 g / L, the total phosphorus concentration was 10 mg / L, the concentration of NaHCO3 was 0.1 g / L, the concentration of MgCl2·6H2O was 0.1 g / L, and the concentration of FeSO4·7H2O was 0.005 g / L.

[0117] (2) Take 1000 mL of synthetic sewage and add it to a 1000 mL conical flask, add the activated sludge suspension, and finally cover the conical flask with a rubber stopper and seal it. Punch a hole in the rubber stopper and insert it into a glass tube with a diameter of 0.8 cm. At the same time, connect the glass tube to the rubber tube and fasten the rubber stopper.

[0118] (3) Nitrogen was introduced into the conical flask through the rubber tube for 15 min, and the rubber tube was sealed with a water stop clamp. The conical flask was then placed in a constant temperature shaker, the temperature was set to 30°C, the speed was set to 150 rpm, and sampling was performed at a fixed time. When sampling, 5 mL was extracted using a disposable syringe, and the nitrate nitrogen and total phosphorus contents of the sample were quickly determined after passing through a 0.45 μm filter membrane, and the nitrogen removal rate and total phosphorus removal rate were calculated.

[0119] After testing, the nitrogen removal rates were 7.3%, 10.4% and 20.2% at 30 minutes, 2 hours and 98 hours of reaction respectively, and there was almost no phosphorus removal effect.

[0120] The above embodiments are only for the purpose of clearly illustrating the embodiments, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method, characterized in that: include: Taking elemental sulfur powder, a divalent iron source and activated carbon powder, placing them in a ball mill for 2 to 4 hours to obtain a powdered composite material; heating and melting the powdered composite material to obtain a molten composite material; The molten composite material is first granulated and then cooled, or the molten composite material is directly cooled and solidified and then crushed to obtain the sulfide-iron-based autotrophic denitrification filler; The total mass percentage of the elemental sulfur powder and the divalent iron source is 80% to 90%, the mass percentage of the activated carbon powder is 10% to 20%; and the mass ratio of the elemental sulfur powder to the divalent iron source is 1:1 to 7:

3.

2. The method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method as claimed in claim 1, characterized in that: The mass ratio of the elemental sulfur powder to the divalent iron source is 7:

3.

3. The method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method as claimed in claim 1, characterized in that: The ferrous iron source is selected from ferrous carbonate and / or ferrous sulfide.

4. The method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method as claimed in claim 1, characterized in that: The step of heating and melting the powdery composite material specifically includes heating the powdery composite material to 120° C. to 140° C. to melt it.

5. The method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method as claimed in claim 1, characterized in that: The rotation speed of the ball mill is 200-600 rpm.

6. The method for preparing ferrous sulfide-based autotrophic denitrification filler by mechanochemical method as claimed in claim 1, characterized in that: The rotation speed of the ball mill was 400 rpm.

7. Use of the sulfide-iron-based autotrophic denitrification filler prepared by the method according to any one of claims 1 to 5 in a denitrification and phosphorus removal process.

8. The use according to claim 7, characterized in that: The denitrification and phosphorus removal process is for denitrification and phosphorus removal of effluent from a secondary sedimentation tank of a sewage treatment plant, an artificial wetland or industrial wastewater.

9. The use according to claim 7, characterized in that: The dosage of the sulfide-iron-based autotrophic denitrification filler is 20-40 g / L.

Citation Information

Patent Citations

  • Preparation method and application of efficient denitrification composite filler

    CN114573103A

  • Denitrification biological filler based on iron-carbon micro-electrolysis as well as preparation method and application of denitrification biological filler

    CN118026388A

  • Preparation method and application of nitrogen and phosphorus removal filler

    CN118239593A

  • Method for preparing autotrophic synchronous nitrogen and phosphorus removal agent through mechanochemical activation of iron sulfide and application method of autotrophic synchronous nitrogen and phosphorus removal agent

    CN118255466A

  • A mechanochemical process to produce exfoliated nanoparticles

    IN202027005960A

Cited By

  • Composite functional material for accelerating granulation of aerobic sludge as well as preparation method and application of composite functional material

    CN120328731A