Dry strength agent and preparation method thereof
By simplifying the preparation process of dry strengthening agents and using specific raw materials and reaction steps, the existing dry strengthening agents have been solved, and the cost reduction and effect improvement have been achieved, and the production process has been simplified.
Patent Information
- Application Number
- CN202410926222.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing dry strength agent has relatively poor use effect and the preparation process is complex, so it cannot reduce production costs through simplified processes, resulting in high production costs and affecting the application efficiency of dry strength agent.
A dry strength agent and its preparation method are adopted, and the raw materials include acrylamide, methacryloyloxyethyltrimethylammonium chloride, dimethylammonium methacrylate, itaconic acid, sodium methylsulfonate, N ,N-dimethacrylamide, chelating agent, sulfuric acid, ammonium persulfate, sodium sulfite, fungicide and defoaming agent, simplify the preparation process through specific reaction steps and process flows, and reduce production costs.
The preparation process is simplified, the production cost is reduced, and the use effect of dry strength agent is improved, the production process is simplified, the production cost is significantly reduced, and the application efficiency of the product is improved.
Smart Images

Figure CN118878740A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pulp additives, in particular to a dry strength agent and a preparation method thereof. Background Art
[0002] Dry strength agents are an important class of chemicals used in the papermaking industry to increase paper strength. Many water-soluble polymers that can form hydrogen bonds with fibers can become dry strength agents. Dry strength agents are usually used to compensate for the decrease in paper strength caused by the addition of fillers or low-grade fibers (such as recycled fibers). Most natural and synthetic dry strength agents are hydrophilic polymers. These polymers are dispersed between fibers to increase the number of bonds between fibers, thereby achieving the purpose of improving paper strength. Most dry strength agents contain cationic groups attached to the main chain ring, which increases the binding force between the polymer and the fiber and improves the retention of the polymer. Commonly used dry strength agents include natural polymers such as starch and its modified products (such as cationic starch, anionic starch), synthetic polymers such as polyacrylamide, glyoxal polyacrylamide and polyvinyl alcohol, and other water-soluble natural product dry strength agents. From the characteristics of their molecular structure, dry strength agents are mostly high molecular polymers containing multiple hydroxyls, which is the basis for the formation of hydrogen bonds with cellulose molecules. The hydrogen bond-forming groups in the dry strength agent molecules form hydrogen bonds with the hydroxyls on the fiber surface. For example, the free glucose hydroxyl groups of starch participate in the formation of hydrogen bonds between cellulose molecules on the fiber surface, so starch increases the bonding force of internal fibers and increases the number of hydrogen bonds on the natural bonding surface between two bundles of fibers. At the same time, the dry strength agent has a certain improvement effect on the paper sheet forming process. The dry strength agent plays the role of a high-efficiency dispersant, that is, the dry strength agent makes the fiber distribution in the pulp more uniform, provides more bonding between fibers and between fibers and polymers, thereby improving the dry strength.
[0003] The current dry strength agent has a relatively poor effect and a complicated preparation process. It is impossible to reduce the production cost by simplifying the preparation process of the dry strength agent, and it is impossible to achieve the purpose of both ensuring the effect of the dry strength agent and saving a lot of production costs, which brings great inconvenience to the production of dry strength agents. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a dry strength agent and a preparation method thereof, which solves the problem that the existing dry strength agent has a relatively poor use effect and a complicated preparation process, and cannot reduce the production cost by simplifying the preparation process of the dry strength agent, and cannot achieve the purpose of both ensuring the use effect of the dry strength agent and saving a large amount of production cost.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical scheme: a dry strength agent, whose raw materials include, by weight: 30-40 parts of acrylamide, 5-10 parts of methacryloyloxyethyltrimethylammonium chloride, 5-10 parts of dimethylaminoethyl methacrylate, 3-5 parts of itaconic acid, 3-5 parts of sodium methacrylic acid sulfonate, 5-10 parts of N,N-dimethylacrylamide, 5-10 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3-5 parts of chelating agent, 1-3 parts of sulfuric acid, 3-5 parts of ammonium persulfate, 1-3 parts of sodium sulfite, 1-3 parts of bactericide, 1-3 parts of defoaming agent and 30-40 parts of water.
[0008] Preferably, the raw materials include, by weight: 35 parts of acrylamide, 7 parts of methacryloyloxyethyltrimethylammonium chloride, 7 parts of dimethylaminoethyl methacrylate, 4 parts of itaconic acid, 4 parts of sodium methacrylic acid sulfonate, 7 parts of N,N-dimethylacrylamide, 7 parts of 2-acrylamido-2-methylpropane sulfonic acid, 4 parts of chelating agent, 2 parts of sulfuric acid, 4 parts of ammonium persulfate, 2 parts of sodium sulfite, 2 parts of bactericide, 2 parts of defoaming agent and 35 parts of water.
[0009] Preferably, the raw materials include, by weight: 30 parts of acrylamide, 5 parts of methacryloyloxyethyltrimethylammonium chloride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of itaconic acid, 3 parts of sodium methacrylic acid sulfonate, 5 parts of N,N-dimethylacrylamide, 5 parts of 2-acrylamido-2-methylpropane sulfonic acid, 3 parts of chelating agent, 1 part of sulfuric acid, 3 parts of ammonium persulfate, 1 part of sodium sulfite, 1 part of bactericide, 1 part of defoaming agent and 30 parts of water.
[0010] Preferably, the raw materials include, by weight: 40 parts of acrylamide, 10 parts of methacryloyloxyethyltrimethylammonium chloride, 10 parts of dimethylaminoethyl methacrylate, 5 parts of itaconic acid, 5 parts of sodium methacrylic acid sulfonate, 10 parts of N,N-dimethylacrylamide, 10 parts of 2-acrylamido-2-methylpropanesulfonic acid, 5 parts of chelating agent, 3 parts of sulfuric acid, 5 parts of ammonium persulfate, 3 parts of sodium sulfite, 3 parts of bactericide, 3 parts of defoaming agent and 40 parts of water.
[0011] Preferably, the fungicide is one of benzisothiazolinone or N-phthalimide.
[0012] Preferably, the defoaming agent is one of polydimethylsiloxane or polyether-modified polysiloxane.
[0013] The present invention also provides a method for preparing a dry strength agent, which specifically comprises the following steps:
[0014] S1. Prepare materials: add water (transported by pipeline), acrylamide, methacryloyloxyethyl trimethylammonium chloride, dimethylaminoethyl methacrylate, itaconic acid, sodium methacrylic acid sulfonate, N,N-dimethylacrylamide, and chelating agent to the reactor in sequence, and add sulfuric acid to adjust the pH value to the process requirements;
[0015] S2, heating the kettle: after reaching 90°C, add chelating agent (solid feeder) and ammonium persulfate, replace the air in the kettle with nitrogen, and after the reaction starts, slowly introduce cooling water, and control the temperature to rise evenly by adjusting the cooling water speed;
[0016] S3, secondary polymerization: after the reaction in step S2 is completed, a mixture of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, methacryloyloxyethyl dimethylbenzyl ammonium chloride, N,N-dimethylacrylamide and itaconic acid is added dropwise into the reaction kettle to carry out secondary polymerization;
[0017] S4, cross-linking: After the reaction of the insulation step S3 is completed, continue to add ammonium persulfate (solid feeder), and when the product viscosity reaches the required level, add sodium sulfite as a stopper, and add adjustment water, bactericide and defoamer;
[0018] S5. Filtration and packaging: Cool down, filter and discharge the material. Use a closed filter to produce a small amount of filter residue, backwash to discharge the residue, and collect and bag the waste residue immediately on site. The filtered product is transported to the finished product tank area through a pipeline. The product is filled using a semi-automatic filling line, and a sealing cover and exhaust device are set on the packaging barrel mouth.
[0019] Preferably, in step S4, the total monomer content is within 1000 ppm when the product viscosity reaches the required level.
[0020] (III) Beneficial effects
[0021] The present invention provides a dry strength agent and a preparation method thereof. Compared with the prior art, the dry strength agent and the preparation method thereof have the following beneficial effects: the raw materials of the dry strength agent and the preparation method thereof include, by weight, 30-40 parts of acrylamide, 5-10 parts of methacryloyloxyethyl trimethyl ammonium chloride, 5-10 parts of dimethylaminoethyl methacrylate, 3-5 parts of itaconic acid, 3-5 parts of sodium methacrylic acid sulfonate, 5-10 parts of N,N-dimethylacrylamide, 5-10 parts of 2-acrylamide-2-methylpropanesulfonic acid, 3-5 parts of chelating agent, 1-3 parts of sulfuric acid, 3-5 parts of ammonium persulfate, 1-3 parts of sodium sulfite, 1-3 parts of bactericide, 1-3 parts of defoaming agent and 30-40 parts of water, which can reduce the production cost by simplifying the preparation process of the dry strength agent, and well achieve the purpose of both ensuring the use effect of the dry strength agent and saving a large amount of production cost, greatly improving the use effect, and well reducing the preparation process, thereby greatly facilitating people's production of the dry strength agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a process flow chart of the preparation process. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] See also Figure 1 The embodiments of the present invention provide three technical solutions: a dry strength agent and a preparation method thereof, specifically including the following embodiments:
[0025] Embodiment 1: A dry strength agent, whose raw materials include by weight: 35 parts of acrylamide, 7 parts of methacryloyloxyethyltrimethylammonium chloride, 7 parts of dimethylaminoethyl methacrylate, 4 parts of itaconic acid, 4 parts of sodium methacrylic acid sulfonate, 7 parts of N,N-dimethylacrylamide, 7 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of chelating agent, 2 parts of sulfuric acid, 4 parts of ammonium persulfate, 2 parts of sodium sulfite, 2 parts of bactericide, 2 parts of defoamer and 35 parts of water, wherein the bactericide is benzisothiazolinone and the defoamer is polydimethylsiloxane.
[0026] The present invention also provides a method for preparing a dry strength agent, which specifically comprises the following steps:
[0027] S1. Material preparation: water (delivered by pipeline), acrylamide (delivered by pipeline), methacryloyloxyethyl trimethyl ammonium chloride (delivered by material pump), dimethylaminoethyl methacrylate (delivered by material pump), itaconic acid (solid feeder), sodium methacrylic acid (solid feeder), N,N-dimethylacrylamide (delivered by material pump), and chelating agent (solid feeder) are sequentially added into the reactor, and sulfuric acid (delivered by pipeline) is added to adjust the pH value to the process requirements;
[0028] S2, heating the kettle: after reaching 90°C, add chelating agent (solid feeder) and ammonium persulfate (solid feeder), replace the air in the kettle with nitrogen, and after the reaction starts, slowly introduce cooling water (pipeline transportation), and control the temperature to rise evenly by adjusting the speed of cooling water;
[0029] S3, secondary polymerization: after the reaction in step S2 is completed, a mixture of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, methacryloyloxyethyl dimethylbenzyl ammonium chloride, N,N-dimethylacrylamide, and itaconic acid (pre-configured in a dropping tank) is added dropwise into the reaction kettle to carry out secondary polymerization;
[0030] S4, cross-linking: After the reaction of the insulation step S3 is completed, continue to add ammonium persulfate (solid feeder), and when the product viscosity reaches the required level, add sodium sulfite (solid feeder) as a stopper, and add adjustment water (pipeline delivery), bactericide (material pump delivery) and defoamer (material pump delivery), and when the product viscosity reaches the required level, the total monomer content is within 1000ppm;
[0031] S5. Filtration and packaging: Cool down, filter and discharge the material. Use a closed filter to produce a small amount of filter residue, backwash to discharge the residue, and collect and bag the waste residue immediately on site. The filtered product is transported to the finished product tank area through a pipeline. The product is filled using a semi-automatic filling line, and a sealing cover and exhaust device are set on the packaging barrel mouth.
[0032] Embodiment 2: A dry strength agent, whose raw materials include by weight: 30 parts of acrylamide, 5 parts of methacryloyloxyethyltrimethylammonium chloride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of itaconic acid, 3 parts of sodium methacrylic acid sulfonate, 5 parts of N,N-dimethylacrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3 parts of chelating agent, 1 part of sulfuric acid, 3 parts of ammonium persulfate, 1 part of sodium sulfite, 1 part of bactericide, 1 part of defoamer and 30 parts of water, wherein the bactericide is N-phthalimide and the defoamer is polyether modified polysiloxane.
[0033] The present invention also provides a method for preparing a dry strength agent, which specifically comprises the following steps:
[0034] S1. Material preparation: water (delivered by pipeline), acrylamide (delivered by pipeline), methacryloyloxyethyl trimethyl ammonium chloride (delivered by material pump), dimethylaminoethyl methacrylate (delivered by material pump), itaconic acid (solid feeder), sodium methacrylic acid (solid feeder), N,N-dimethylacrylamide (delivered by material pump), and chelating agent (solid feeder) are sequentially added into the reactor, and sulfuric acid (delivered by pipeline) is added to adjust the pH value to the process requirements;
[0035] S2, heating the kettle: after reaching 90°C, add chelating agent (solid feeder) and ammonium persulfate (solid feeder), replace the air in the kettle with nitrogen, and after the reaction starts, slowly introduce cooling water (pipeline transportation), and control the temperature to rise evenly by adjusting the speed of cooling water;
[0036] S3, secondary polymerization: after the reaction in step S2 is completed, a mixture of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, methacryloyloxyethyl dimethylbenzyl ammonium chloride, N,N-dimethylacrylamide, and itaconic acid (pre-configured in a dropping tank) is added dropwise into the reaction kettle to carry out secondary polymerization;
[0037] S4, cross-linking: After the reaction of the insulation step S3 is completed, continue to add ammonium persulfate (solid feeder), and when the product viscosity reaches the required level, add sodium sulfite (solid feeder) as a stopper, and add adjustment water (pipeline delivery), bactericide (material pump delivery) and defoamer (material pump delivery), and when the product viscosity reaches the required level, the total monomer content is within 1000ppm;
[0038] S5. Filtration and packaging: Cool down, filter and discharge the material. Use a closed filter to produce a small amount of filter residue, backwash to discharge the residue, and collect and bag the waste residue immediately on site. The filtered product is transported to the finished product tank area through a pipeline. The product is filled using a semi-automatic filling line, and a sealing cover and exhaust device are set on the packaging barrel mouth.
[0039] Example 3: A dry strength agent, whose raw materials include, by weight: 40 parts of acrylamide, 10 parts of methacryloyloxyethyltrimethylammonium chloride, 10 parts of dimethylaminoethyl methacrylate, 5 parts of itaconic acid, 5 parts of sodium methacrylic acid sulfonate, 10 parts of N,N-dimethylacrylamide, 10 parts of 2-acrylamido-2-methylpropanesulfonic acid, 5 parts of chelating agent, 3 parts of sulfuric acid, 5 parts of ammonium persulfate, 3 parts of sodium sulfite, 3 parts of bactericide, 3 parts of defoamer and 40 parts of water, the bactericide is benzisothiazolinone, and the defoamer is polydimethylsiloxane.
[0040] The present invention also provides a method for preparing a dry strength agent, which specifically comprises the following steps:
[0041] S1. Material preparation: water (delivered by pipeline), acrylamide (delivered by pipeline), methacryloyloxyethyl trimethyl ammonium chloride (delivered by material pump), dimethylaminoethyl methacrylate (delivered by material pump), itaconic acid (solid feeder), sodium methacrylic acid (solid feeder), N,N-dimethylacrylamide (delivered by material pump), and chelating agent (solid feeder) are sequentially added into the reactor, and sulfuric acid (delivered by pipeline) is added to adjust the pH value to the process requirements;
[0042] S2, heating the kettle: after reaching 90°C, add chelating agent (solid feeder) and ammonium persulfate (solid feeder), replace the air in the kettle with nitrogen, and after the reaction starts, slowly introduce cooling water (pipeline transportation), and control the temperature to rise evenly by adjusting the speed of cooling water;
[0043] S3, secondary polymerization: after the reaction in step S2 is completed, a mixture of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, methacryloyloxyethyl dimethylbenzyl ammonium chloride, N,N-dimethylacrylamide, and itaconic acid (pre-configured in a dropping tank) is added dropwise into the reaction kettle to carry out secondary polymerization;
[0044] S4, cross-linking: After the reaction of the insulation step S3 is completed, continue to add ammonium persulfate (solid feeder), and when the product viscosity reaches the required level, add sodium sulfite (solid feeder) as a stopper, and add adjustment water (pipeline delivery), bactericide (material pump delivery) and defoamer (material pump delivery), and when the product viscosity reaches the required level, the total monomer content is within 1000ppm;
[0045] S5. Filtration and packaging: Cool down, filter and discharge the material. Use a closed filter to produce a small amount of filter residue, backwash to discharge the residue, and collect and bag the waste residue immediately on site. The filtered product is transported to the finished product tank area through a pipeline. The product is filled using a semi-automatic filling line, and a sealing cover and exhaust device are set on the packaging barrel mouth.
[0046] In the embodiments of the present invention, the main production equipment for preparing the dry strength agent is shown in Table 1.
[0047] Table 1 Main production equipment for dry strength agent preparation
[0048]
[0049]
[0050] In summary, the present invention can reduce the production cost by simplifying the preparation process of the dry strength agent, and well achieves the purpose of both ensuring the use effect of the dry strength agent and saving a lot of production costs, greatly improving the use effect, and well shortening the preparation process, thereby greatly facilitating people's production of the dry strength agent.
[0051] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0052] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A dry strength agent, characterized in that: The raw materials include, by weight, 30-40 parts of acrylamide, 5-10 parts of methacryloyloxyethyltrimethylammonium chloride, 5-10 parts of dimethylaminoethyl methacrylate, 3-5 parts of itaconic acid, 3-5 parts of sodium methacrylic acid sulfonate, 5-10 parts of N,N-dimethylacrylamide, 5-10 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3-5 parts of chelating agent, 1-3 parts of sulfuric acid, 3-5 parts of ammonium persulfate, 1-3 parts of sodium sulfite, 1-3 parts of bactericide, 1-3 parts of defoaming agent and 30-40 parts of water.
2. A dry strength agent according to claim 1, characterized in that: The raw materials include, by weight: 35 parts of acrylamide, 7 parts of methacryloyloxyethyltrimethylammonium chloride, 7 parts of dimethylaminoethyl methacrylate, 4 parts of itaconic acid, 4 parts of sodium methacrylic acid sulfonate, 7 parts of N,N-dimethylacrylamide, 7 parts of 2-acrylamido-2-methylpropane sulfonic acid, 4 parts of chelating agent, 2 parts of sulfuric acid, 4 parts of ammonium persulfate, 2 parts of sodium sulfite, 2 parts of bactericide, 2 parts of defoaming agent and 35 parts of water.
3. A dry strength agent according to claim 1, characterized in that: The raw materials include, by weight: 30 parts of acrylamide, 5 parts of methacryloyloxyethyltrimethylammonium chloride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of itaconic acid, 3 parts of sodium methacrylic acid sulfonate, 5 parts of N,N-dimethylacrylamide, 5 parts of 2-acrylamido-2-methylpropane sulfonic acid, 3 parts of chelating agent, 1 part of sulfuric acid, 3 parts of ammonium persulfate, 1 part of sodium sulfite, 1 part of bactericide, 1 part of defoaming agent and 30 parts of water.
4. A dry strength agent according to claim 1, characterized in that: The raw materials include, by weight: 40 parts of acrylamide, 10 parts of methacryloyloxyethyltrimethylammonium chloride, 10 parts of dimethylaminoethyl methacrylate, 5 parts of itaconic acid, 5 parts of sodium methacrylic acid sulfonate, 10 parts of N,N-dimethylacrylamide, 10 parts of 2-acrylamido-2-methylpropane sulfonic acid, 5 parts of chelating agent, 3 parts of sulfuric acid, 5 parts of ammonium persulfate, 3 parts of sodium sulfite, 3 parts of bactericide, 3 parts of defoaming agent and 40 parts of water.
5. A dry strength agent according to any one of claims 1 to 4, characterized in that: The bactericide is one of benzisothiazolinone and N-phthalimide.
6. A dry strength agent according to any one of claims 1 to 4, characterized in that: The defoaming agent is one of polydimethylsiloxane or polyether-modified polysiloxane.
7. A method for preparing the dry strength agent according to any one of claims 1 to 4, characterized in that: The specific steps include: S1. Prepare materials: add water (transported by pipeline), acrylamide, methacryloyloxyethyl trimethylammonium chloride, dimethylaminoethyl methacrylate, itaconic acid, sodium methacrylic acid sulfonate, N,N-dimethylacrylamide, and chelating agent to the reactor in sequence, and add sulfuric acid to adjust the pH value to the process requirements; S2, heating the kettle: after reaching 90°C, add chelating agent (solid feeder) and ammonium persulfate, replace the air in the kettle with nitrogen, and after the reaction starts, slowly introduce cooling water, and control the temperature to rise evenly by adjusting the cooling water speed; S3, secondary polymerization: after the reaction in step S2 is completed, a mixture of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, methacryloyloxyethyl dimethylbenzyl ammonium chloride, N,N-dimethylacrylamide and itaconic acid is added dropwise into the reaction kettle to carry out secondary polymerization; S4, cross-linking: After the reaction of the insulation step S3 is completed, continue to add ammonium persulfate (solid feeder), and when the product viscosity reaches the required level, add sodium sulfite as a stopper, and add adjustment water, bactericide and defoamer; S5. Filtration and packaging: Cool down, filter and discharge the material. Use a closed filter to produce a small amount of filter residue, backwash to discharge the residue, and collect and bag the waste residue immediately on site. The filtered product is transported to the finished product tank area through a pipeline. The product is filled using a semi-automatic filling line, and a sealing cover and exhaust device are set on the packaging barrel mouth.
8. The method for preparing a dry strength agent according to claim 7, characterized in that: In the step S4, when the viscosity of the product reaches the required level, the total monomer content is within 1000 ppm.